GATE Production and Industrial Engineering (PI): General Engineering (materials, iron-carbon diagram, strength of materials, theory of machines, machine design, thermodynamics, fluid mechanics, heat transfer), previous-year questions solved
Every General Engineering question from the GATE PI papers of 2024, 2025 and 2026, solved: materials and the iron-carbon diagram, trusses, beams, pressure vessels and failure theories, mechanisms, belts, bolts and gears, air-standard cycles, pipe flow and heat transfer. Every answer matches the official key and was recomputed in code.
Questions from official GATE PI papers (IISc Bengaluru 2024, IIT Roorkee 2025, IIT Guwahati 2026); solutions by Skill-Lync. · Updated 20 Nov 2026 · 16 of 30 questions on this page
Which pure metal is hexagonal close packed (HCP) at room temperature: Mg, Fe, Al or Cu
- (A)Magnesium
- (B)Iron
- (C)Aluminium
- (D)Copper
Answer: (A) Official key: A
- Most common metals crystallise in one of three structures: body-centred cubic (BCC), face-centred cubic (FCC) and hexagonal close packed (HCP). The structure at room temperature has to be remembered; it is a property of the atom and not something to calculate.
- (A) Magnesium: HCP. Others in the HCP group are zinc, titanium (below 882 °C), cadmium and cobalt (at room temperature).
- (B) Iron: BCC at room temperature (alpha iron, ferrite). It turns FCC (gamma iron, austenite) only above 912 °C.
- (C) Aluminium: FCC. (D) Copper: FCC.
- Only magnesium is HCP: (A).
Check: the four metals were stored with their room-temperature structures and only magnesium matched HCP. Trap: choosing iron because it is the most familiar metal; iron is BCC at room temperature and its FCC form exists only above 912 °C.
HCP metals such as magnesium and titanium have few slip systems at room temperature, so they are formed warm or hot, and die-cast magnesium parts are cast rather than cold pressed. FCC metals such as aluminium and copper have many slip systems and cold form easily into sheet and wire.
Mild steel in a uniaxial tensile test: which of the four statements are true
- (A)The engineering stress-strain curve is linear within the elastic limit.
- (B)The specimen fails in cup and cone type fracture.
- (C)The true stress is always more than the engineering stress at any finite strain.
- (D)The specimen does not regain its original dimensions after complete unloading from an initial stress above the yield stress.
Answer: (B) and (C) and (D) Official key: B;C;D
- The test pulls a bar and records engineering stress against engineering strain using the original area and length.
- (A) False. The curve is straight only up to the proportional limit. Mild steel has an elastic limit just above it, where the curve bends slightly although the bar still recovers fully. So the statement as worded is not strictly true, and the official key leaves (A) out.
- (B) True. Mild steel is ductile, so it necks, a crack starts inside the neck and spreads, and the fracture surfaces form a cup and a cone.
- (C) True. Volume stays constant in plastic flow, so the true stress is . The factor is above 1 for any strain above zero, so true stress is always higher than engineering stress.
- (D) True. Beyond the yield stress part of the strain is plastic and stays on unloading as a permanent set.
- The true statements are (B), (C) and (D).
Check: each statement was stored with a reason, and the true-stress relation was scanned for strains from 0.000001 to 0.2 at stresses of 250 and 400 MPa: every time. Trap: marking (A) true; the words matter, since the straight line ends at the proportional limit and not at the elastic limit.
Tensile tests on mild steel bar and plate are run on every incoming heat to check yield and ultimate strength against the certificate. A cup and cone fracture with visible necking tells the inspector that the bar was ductile, while a flat, shiny fracture with no necking is a warning sign.
Steel with 1.2 wt % carbon cooled from 1000 C: fraction of pro-eutectoid cementite
- (A)0.07
- (B)0.93
- (C)0.18
- (D)0.12
Answer: (A) Official key: A
- Steel with 1.2 % C is hypereutectoid (above 0.77 % C). Cooled slowly from 1000 °C (all austenite) it reaches the line where cementite starts to separate along the grain boundaries. That cementite, formed above 727 °C, is pro-eutectoid cementite. The remaining austenite reaches 0.77 % C and turns to pearlite at 727 °C.
- Just above 727 °C the two phases are austenite (0.77 % C) and cementite FeC (6.67 % C). The lever rule gives the cementite fraction as the distance from the alloy to the austenite end, divided by the full tie line.
- 0.07, option (A).
- The rest, (0.93), is pearlite.
Check: the lever rule was computed with exact fractions and rounded to 2 decimals; only (A) = 0.07 agrees. The other options are slips: 0.93 is the pearlite fraction, 0.18 is (the cementite fraction with the lever taken from zero carbon, not from 0.77 %) and 0.12 is .
Heat treatment shops know that high-carbon tool steel cooled slowly from the austenite range forms a brittle cementite network on the grain boundaries. Spheroidising anneals and controlled cooling are used to avoid it before machining and hardening.
Atomic packing factor of a body centred cubic structure
- (A)0.34
- (B)0.52
- (C)0.68
- (D)0.74
Answer: (C) Official key: C
- The atomic packing factor (APF) is the fraction of the unit cell volume filled by atoms, treated as hard touching spheres: APF = (atoms per cell volume of one atom) / volume of the cell.
- A BCC cell has 8 corner atoms shared by 8 cells (1 atom) plus 1 atom at the centre: 2 atoms per cell. The spheres touch along the body diagonal, which is long and holds 4 radii, so .
- APF , so option (C).
- The other options are the neighbours on the packing ladder: simple cubic 0.52 (B), diamond cubic 0.34 (A), and FCC or HCP 0.74 (D).
Trap: 0.74 is the famous maximum, and it belongs to the close-packed structures FCC and HCP. BCC is a little looser, so metals such as iron below 912 C, chromium and tungsten have 32 % of the volume empty.
Packing density explains why iron changes volume when it moves between BCC and FCC during heat treatment, and why FCC steels dissolve more carbon. Heat treatment shops rely on this when they plan quench distortion and retained austenite.
Fraction of eutectoid ferrite in 0.7 wt % carbon steel cooled slowly below 723 C
Answer: 0.74 Official key: 0.72 to 0.76
- The lever rule gives phase fractions: the fraction of a phase is the length of the tie line on the far side of the alloy composition, divided by the whole tie line. A 0.7 % C steel is hypoeutectoid (below 0.83 % C): slow cooling first forms proeutectoid ferrite, and the rest of the austenite turns into pearlite at 723 C.
- Pearlite fraction (austenite just above 723 C, tie line 0.022 to 0.83): . The proeutectoid ferrite is the rest: .
- Pearlite is a mixture of ferrite and cementite in its own proportion (tie line 0.022 to 6.67): ferrite share of pearlite .
- Eutectoid ferrite (the ferrite inside the pearlite) .
- Check: eutectoid ferrite + proeutectoid ferrite , which equals the total ferrite from one lever rule below 723 C, .
Trap: the total ferrite is 0.90, the pearlite is 0.84 and the proeutectoid ferrite is 0.16. All three are outside the key; the question asks only for the ferrite that belongs to the eutectoid reaction.
Heat treatment shops estimate the pearlite and ferrite shares of a medium-carbon steel from its carbon content to predict hardness and strength after annealing or normalising. Metallographers check these fractions against the microstructure under the microscope.
Heat treatment that gives only bainite in a eutectoid plain carbon steel
Which ONE of the following is the corresponding heat treatment method?
- (A)Normalizing
- (B)Annealing
- (C)Martempering
- (D)Austempering
Answer: (D) Official key: D
- Rule: the microstructure of a eutectoid steel depends on how it is cooled from austenite, read on the TTT (time-temperature-transformation) diagram. Slow cooling gives pearlite, a quench below the martensite start temperature gives martensite, and holding at a constant temperature between the pearlite nose and (about 250 to 400 °C) gives bainite, a fine plate of ferrite and carbide.
- (A) Normalizing: air cooling gives fine pearlite. (B) Annealing: furnace cooling gives coarse pearlite. Both are above the nose, so no bainite.
- (C) Martempering: quench to just above , hold briefly only to even out the temperature, then cool through . The result is martensite, not bainite.
- (D) Austempering: quench into a salt bath at 250 to 400 °C and hold until the austenite has fully transformed. The result is 100 % bainite. The answer is (D).
Trap: martempering and austempering both start with an interrupted quench. The difference is the hold: austempering holds long enough to finish the bainite reaction, martempering holds only to equalise the temperature. We stored each treatment with its product and tested every option: only (D) gives bainite alone.
Heat treatment shops austemper springs, clips, chain parts and small gears in salt baths because bainite gives high strength with better toughness and less distortion and cracking than a quenched and tempered martensite.
Name of the iron-carbon alloy with pro-eutectoid ferrite and pearlite at room temperature
Which ONE of the following best describes this Iron-Carbon alloy?
- (A)Hyper-eutectic steel
- (B)Hyper-eutectoid steel
- (C)Hypo-eutectoid steel
- (D)Eutectoid steel
Answer: (C) Official key: C
- Rule: on the iron-carbon diagram the eutectoid point is at 0.77 % carbon and 727 °C. A steel with less carbon is hypo-eutectoid: on cooling, austenite first throws out pro-eutectoid ferrite above 727 °C, then the remaining austenite (now 0.77 % carbon) turns to pearlite just below it. A steel with more carbon is hyper-eutectoid: pro-eutectoid cementite then pearlite.
- The alloy has pro-eutectoid ferrite plus pearlite, so the carbon is below 0.77 %. For example at 0.4 % carbon the lever rule gives of the alloy as pro-eutectoid ferrite, the rest pearlite.
- (B) is out because its pro-eutectoid phase is cementite. (D) is out because a eutectoid steel is 100 % pearlite with no pro-eutectoid phase. (A) is out because hyper-eutectic is a term for cast irons above 4.3 % carbon, not steels.
- So the alloy is a hypo-eutectoid steel, option (C).
Trap: eutectic and eutectoid sound alike. Eutectic is liquid turning to two solids (4.3 % C); eutectoid is solid turning to two solids (0.77 % C). We tested each class on sample carbon contents from 0.1 to 1.2 %: only hypo-eutectoid always gives pro-eutectoid ferrite with pearlite.
Most structural and machine steels (0.1 to 0.6 % carbon) are hypo-eutectoid, and a metallurgist reads their ferrite and pearlite proportions under the microscope to estimate carbon content and strength after rolling, forging or normalizing.
Cantilever of length L with force F at 2L/3 from the wall: deflection at the free end
- (A)
- (B)
- (C)
- (D)
Answer: (B) Official key: B
- Euler-Bernoulli beam theory says the curvature of the beam is . For a cantilever load at distance from the wall, the part of the beam beyond the load carries no moment, so it stays straight at the slope reached under the load.
- Under the load, and the slope is (a cantilever of length with a tip load).
- The free end is a further along a straight line at slope , so .
- Put : and , so , option (B).
Check: the moment for (zero beyond) was integrated twice numerically with and gave against ; the options are , and , so only (B) matches. Trap: using the tip-load formula for a load that is not at the tip; the load at gives less than half of that.
Cantilever deflection checks the sag of a fixture arm, a jib crane boom, a boring bar or a tool overhang under a side load. Designers use the same step, a straight overhang beyond the load at the slope reached under it, to estimate the deflection of a bar loaded part way along.
Square truss with a string diagonal AC, 100 kN at B and F at 60 degrees at C: maximum F in kN
Answer: 200 Official key: 199.95 to 200.05
- A string can only pull: its force is a tension and cannot be negative. If the equations ask for a compression in AC, the string goes slack and the truss collapses. So the largest is the one that brings the string tension down to zero.
- Whole truss: the load at B is 100 kN to the right; at C has components (left) and (down). The roller at D gives a vertical reaction only. Moments about A (side ): , so .
- Horizontal forces: , so .
- Joint D has the roller reaction and members DC (vertical) and DA (horizontal), so DA carries nothing. At joint A, members AB (vertical) and AC (at 45 degrees) meet the pin reaction. The horizontal balance gives , so kN.
- needs kN. The maximum force is kN.
Check: all five member forces and three reactions were solved from the eight joint equations at kN: = 0.00 kN (the string just goes slack), = 0.00 kN, = 0.00 kN, = 173.21 kN, BC = 100.00 kN (compression), CD = 173.21 kN (compression), and AB and DA are zero. At = 150 kN the string tension is 35.4 kN (taut) and at = 250 kN it would have to be -35.4 kN, which a string cannot give. Trap: treating AC as a rigid bar, which would let be any size.
Cable and rod braced frames work the same way: a tie rod or wire diagonal carries tension only, so the designer checks that no brace is asked for compression under any load case. Gantry frames, crane booms and fixture frames with turnbuckle braces are checked this way.
Thin cylindrical air vessel, 1 m radius, 4 mm wall, 100 MPa normal and 40 MPa shear limits: allowable pressure
Answer: 0.32 Official key: 0.31 to 0.33
- A thin-walled cylinder () has a hoop stress around the circumference and a longitudinal stress along the axis. The radial stress is small (from inside to 0 outside) and is taken as zero. So and .
- Normal stress limit: the largest normal stress is the hoop stress, , so MPa.
- Shear stress limit: the absolute maximum shear stress is half the largest difference of the three principal stresses, , and . The largest difference is , so , so MPa. (The in-plane shear is smaller and would allow MPa, but it is not the largest shear on the wall.)
- Both limits must hold, so the smaller one governs: the shear limit gives 0.32 MPa, inside the key range 0.31 to 0.33.
Check: at MPa the stresses are = 80 MPa (below 100) and = 40 MPa, and the maximum shear is 40 MPa, exactly at the limit. Trap: stopping at the normal stress limit, which gives 0.40 MPa and would let the wall shear at 50 MPa, above the 40 MPa allowed.
Compressed air receivers, boilers and hydraulic accumulators are sized from hoop stress, and the design pressure is set by the lower of the normal and shear limits. The relation of pressure times radius over wall thickness is also used to estimate the wall thickness of a pressurised pipe or the burst pressure of a test sample.
Reaction force at A of a beam on a pin and a roller carrying a moment M at C
- (A)
- (B)
- (C)
- (D)
Answer: (A) Official key: A
- Use the equilibrium equations for a body in a plane: and about any point. There is no load along the beam, so there are only two unknowns, the vertical reactions and .
- A pure moment (a couple) adds no force, so gives : the two reactions are equal and opposite and form a couple of their own.
- Moments about A, counter clockwise positive (as drawn): , so (downwards) and (upwards).
- The position of the moment does not appear: a couple has the same moment about every point. So the magnitude of the reaction at A is , option (A).
Trap: the distance is a distractor. It decides where the bending moment diagram jumps by , not the size of the reactions. Check with N m and m: both reactions are 250 N for any .
A moment applied through an offset load on a bracket or a shaft is carried by an equal and opposite pair of support reactions. Fixture designers use this to size the clamps that hold an off-centre part on a table.
Relationship between hoop stress and longitudinal stress in a closed thin-walled cylindrical pressure vessel
- (A)
- (B)
- (C)
- (D)
Answer: (A) Official key: A
- Take a thin cylinder of internal diameter , wall thickness and internal pressure . Cut it along its length and balance one half: the pressure pushes on the projected area , and two wall strips of area resist, so and (hoop stress).
- Cut it across and balance one end: the pressure pushes on the end area , and the ring of area resists, so and (longitudinal stress). The end caps make the vessel closed.
- Divide: , so , option (A). For example MPa, mm, mm gives 50 MPa hoop and 25 MPa longitudinal.
Trap: the hoop stress is the larger one, so a seam that runs along the length of a boiler shell is loaded twice as hard as a girth (circumferential) seam. For a sphere both are .
Pressure vessel and air receiver shells are sized on the hoop stress, which is why longitudinal welds are inspected more strictly than girth welds. Compressed air tanks and hydraulic cylinders in press shops follow the same rule.
Yield strength by the Tresca criterion for principal stresses of 300, 250 and 100 MPa
Answer: 200 Official key: 199 to 201
- The Tresca (maximum shear stress) criterion says a ductile metal yields when the largest shear stress reaches the shear stress at yield in a tension test, .
- The largest shear stress is half of the largest difference of principal stresses: MPa. The middle stress (250 MPa) does not enter.
- At yield , so MPa.
Contrast: the von Mises criterion squares the three differences, , and gives MPa, outside the key. Tresca is the more conservative of the two.
Designers of pressure parts and shafts use the maximum shear criterion because it is simple and errs on the safe side. Press frames and forgings are checked with von Mises when a closer estimate is needed.
Moment about B of a 1000 N force acting at A of a bracket, force at 60 degrees
Answer: 186.6 Official key: 185.0 to 188.0
- The moment of a force about a point is : the position vector from the point to the force's line, crossed with the force. In two dimensions, .
- From the figure, A is 0.1 m to the right of B and 0.2 m above it, so m. The force points up and to the left at above the horizontal: N and N.
- N m. Both components turn the bracket the same way (counter clockwise about B), so their moments add.
- The magnitude is 186.6 N m, inside the key range.
Trap: the signs. Subtracting the 100 N m term gives 13.4 N m. A force that points away from the wall pulls A to the left, so its horizontal component and its vertical component both turn the bracket counter clockwise. Swapping the angle to gives 223.2 N m.
Moments of off-line loads decide the bolt and weld sizes of brackets, fixture arms and tooling plates. A part clamped on one side of a fixture and pulled by the cutting force from the other side is checked this way.
Name of the ratio of hydrostatic stress to volumetric strain
- (A)Bulk modulus
- (B)Compressibility
- (C)Poisson’s ratio
- (D)Young’s modulus
Answer: (A) Official key: A
- Rule: each elastic constant is a stress-to-strain ratio for one loading. Young's modulus is axial stress over axial strain. The bulk modulus is hydrostatic stress (equal pressure in all directions) over volumetric strain . Poisson's ratio is lateral strain over axial strain and has no unit.
- Check from Hooke's law. Take steel, GPa, , under a hydrostatic stress of 100 MPa. Each direction strains by , so the volumetric strain is .
- Ratio , which equals . This is the bulk modulus, option (A).
- (B) Compressibility is the reciprocal, , strain per unit stress. (C) 0.30 is dimensionless. (D) 200 GPa is the axial ratio. Only (A) equals the computed ratio.
Trap: compressibility sounds like the right name but is the inverse of the ratio asked.
The bulk modulus decides how much a liquid or a rubber seal compresses under pressure, which matters for hydraulic press circuits, O-ring grooves, rubber pads in forming dies and pressure vessel fills.
Poisson's ratio from a 3 x 10^-3 mm diameter reduction of a 10 mm bar under 14 kN
If its Young's modulus is 150 GPa, the Poisson's ratio of the material is ______ (rounded off to two decimal places).
Note: Assume .
Answer: 0.25 Official key: 0.22 to 0.28
- Rule: Poisson's ratio is , the lateral strain over the axial strain. In uniaxial tension the axial strain comes from Hooke's law, .
- Area . Stress .
- Axial strain .
- Lateral strain magnitude (the diameter shrinks).
- 0.25.
Check: the value lies in the usual 0.25 to 0.35 band for metals. Common slip: using for the area (forgetting the divide by 4) gives 1.01.
Strain gauge rosettes and extensometers on tensile bars and pressure parts measure axial and lateral strain together to find Poisson's ratio, which feeds the finite element models used for press frames and pressure vessels.