GATE Production and Industrial Engineering (PI): Casting, Forming and Joining (solidification time, gating, risers, shrinkage, rolling, wire drawing, blanking, deep drawing, arc and friction stir welding, brazing, powder metallurgy, polymers and composites), previous-year questions solved

Every Manufacturing Processes I question from the GATE Production and Industrial Engineering papers of 2024, 2025 and 2026, solved: Chvorinov's rule and riser sizing, sprue design without aspiration, shrinkage allowances, centrifugal casting, casting and forming defects, rolling bite and friction, wire drawing with front tension, blanking clearance and force, deep drawing limits, arc welding heat input and the arc characteristic, friction stir welding and brazing, powder densities, polymer extrusion and filament winding. Each answer matches the official key and was recomputed by code with the numbers printed in the paper.

Questions from official GATE PI papers (IISc Bengaluru 2024, IIT Roorkee 2025, IIT Guwahati 2026); solutions by Skill-Lync. · Updated 19 Nov 2026 · 28 questions

GATE 2024 · PI · Q.15MCQ · 1 markCasting: solidification, gating, risers and defects

Cube of side a and cylinder of radius r and length 4r solidify in equal time: find r/a

The solidification time of a cube and a cylinder of the same material, produced through the same sand casting process, is found to be equal. Each side of the cube is , and the radius and the length of the cylinder are and , respectively. If the solidification time is governed by Chvorinov’s equation, then the ratio is
  1. (A)1/3
  2. (B)5/12
  3. (C)7/12
  4. (D)5/9

Answer: (B) Official key: B

  1. Chvorinov’s rule: the time a casting takes to freeze is , where is its volume, the surface through which heat leaves into the mould, and a constant of the metal and mould. The ratio is the modulus. The same metal and the same sand process mean the same , so equal solidification time means equal modulus.
  2. Cube: , , so modulus .
  3. Cylinder (radius , length ): . Every face is in contact with sand, so (curved side plus two end faces). Modulus .
  4. Equate: , so : (B).

Check: each option was put back into the two moduli with exact fractions, and only makes them equal. Trap: leaving out the two end faces of the cylinder, so that , modulus and , which is option (A). Chvorinov counts every surface that touches the mould.

Where this shows up in industry

Foundry engineers compare the modulus of a casting section with the modulus of its riser using this rule, so that the riser freezes later and keeps feeding. A cube or cylinder cast in sand is a standard test shape for checking mould and metal constants.

GATE 2024 · PI · Q.54NAT · 2 marksCasting: solidification, gating, risers and defects

Tapered sprue with zero gauge pressure at point 2 to avoid aspiration: ratio A3/A2

In a sand mold, a sprue of height mm is to be provided for maintaining the molten metal flow rate of mm/s. The height of liquid column above the point 2 is kept constant at mm. The cross-sectional areas of the sprue at points 2 and 3 are and , respectively. The points 1 and 3 are at the atmospheric pressure. Assuming the gauge pressure at point 2 to be zero as the limiting case to prevent aspiration effect, the ratio is __________ . (Rounded off to 2 decimal places)
Sprue in a sand mould: a pouring basin whose free surface is point 1, the sprue entry at point 2 a height hc below it, and the sprue exit at point 3 a further height h2 below point 2; the sprue narrows downwards123hch2molten metalsandmould

Answer: 0.33 Official key: 0.31 to 0.35

  1. The metal falls in the sprue and speeds up. If the sprue had the same area all the way down, the stream would be pulled thin and the pressure at point 2 would drop below atmospheric, sucking air and mould gases into the metal: aspiration. A sprue that narrows downwards keeps the stream full. The limiting design has gauge pressure .
  2. Bernoulli from point 1 (free surface, at rest, atmospheric) to point 2, taken at the sprue entry a height below: . With : .
  3. Bernoulli from point 1 to point 3 (exit, atmospheric), a height below the surface: .
  4. Continuity (the same volume per second at every section): , so .
  5. 0.33, inside the key range 0.31 to 0.35.

Check: with mm/s the speeds are mm/s and mm/s. The flow rate mm/s then gives mm (diameter 42.6 mm) and mm (diameter 24.6 mm), which does not change the ratio. Scanning from 0.1 to 1, the pressure at point 2 crosses zero at 0.333; a straight sprue () gives a gauge pressure of , a suction. Trap: inverting the ratio (exit area over entry area is smaller than 1 because the stream speeds up, so the sprue must narrow); would make the sprue widen downwards and invite aspiration.

Where this shows up in industry

Foundry designers taper every sprue and put a well and a choke at its foot, so the stream stays full, air is not drawn in and the mould fills without oxide films. The area at each level follows the inverse square root of the head at that level.

GATE 2025 · PI · Q.23MCQ · 1 markCasting: solidification, gating, risers and defects

Casting defect caused by supplying the molten metal through two gates

Which one of the following casting defects is caused due to the supply of the molten metal through two gates?
  1. (A)Cold shut
  2. (B)Shift
  3. (C)Pin hole
  4. (D)Rat tail

Answer: (A) Official key: A

  1. With two gates the metal enters the cavity as two streams that meet part-way. If they have cooled too much when they meet, the surfaces do not fuse and a seam, or cold shut, remains.
  2. (B) Shift is a mismatch between cope and drag halves. (C) Pin holes are tiny gas holes from dissolved or trapped gas. (D) Rat tail is a shallow line on the casting surface caused by sand expansion buckling the mould face.
  3. Only the cold shut is caused by two metal streams meeting, so the answer is (A).

Check: a cold shut is also caused by a low pouring temperature or a thin section, but here the clue is the two gates.

Where this shows up in industry

Foundries cure cold shuts by raising pouring temperature, speeding up filling, moving or merging gates so streams do not meet late, and avoiding thin long flow paths. Wheel and housing castings often show them where two fronts meet.

GATE 2025 · PI · Q.53NAT · 2 marksCasting: solidification, gating, risers and defects

Side of the cubical pattern for an 80 mm cube casting with 4.5 percent and 2 percent shrinkages

In casting a cube of 80 mm side, the volumetric shrinkages due to solidification and solid contraction are 4.5% and 2%, respectively. Assume uniform cooling in all directions. The side (in mm) of the cubical pattern for getting the required size casting is________. (Rounded off to two decimal places)

Answer: 81.70 mm Official key: 81.50 to 82.50

  1. The pattern must be larger than the casting by the total shrinkage the metal will suffer. The two volumetric shrinkages are added: percent.
  2. Required casting volume . Pattern volume .
  3. For uniform cooling the cube stays a cube, so the pattern side is mm.
  4. Other accepted readings land in the key range 81.50 to 82.50: compounding the two shrinkages gives 81.79 mm, and a linear 6.5/3 percent allowance gives 81.73 mm.

Trap: subtracting the shrinkage, mm, makes the pattern smaller than the casting, which is the wrong direction.

Where this shows up in industry

Pattern makers add a shrinkage allowance to every dimension, often 1 to 2 percent for cast iron and steel and more for aluminium, so the cold casting matches the drawing. Solidification shrinkage is normally fed by the riser rather than taken in the pattern size.

GATE 2025 · PI · Q.54NAT · 2 marksCasting: solidification, gating, risers and defects

Centre-line feeding resistance in percent from the solidification start and finish times

The solidification of a casting starts at 10 AM. However, the solidification of the molten metal at the center-line of the mold starts at 10:03 AM and ends at 10:10 AM. The casting is considered solidified completely when the solidification is completed at the center-line of the mold. The center-line feeding resistance (CFR) in percentage is________. (Answer in integer)

Answer: 70 percent Official key: 70 to 70

  1. Centre-line feeding resistance measures how late in the freezing time the centre-line starts to solidify, which is when feed metal can no longer reach it. It is , where and are the times the centre-line starts and finishes solidifying, counted from the start of solidification of the casting.
  2. The casting starts at 10:00, so min and min (casting complete when the centre-line is complete).
  3. percent.

Trap: percent is the fraction of the time before the centre-line starts, which is the opposite measure.

Where this shows up in industry

A high centre-line feeding resistance means a wide mushy zone in alloys with a long freezing range, and such castings are prone to centre-line shrinkage porosity. Foundries add chills, change the riser or pick narrower-range alloys when it is high.

GATE 2026 · PI · Q.25MSQ · 1 markCasting: solidification, gating, risers and defects

Which tube cross-sections can be produced by true centrifugal casting

Which ONE or MORE among the following tube cross-sections shown can be produced by true centrifugal casting method?

Note: The cross-sections shown are perpendicular to the axis of rotation. Figures are not to scale.

  1. (A)Pentagonal outer outline with a pentagonal bore
  2. (B)Heptagonal outer outline with a circular bore
  3. (C)Pentagonal outer outline with a circular bore
  4. (D)Circular outer outline with a heptagonal bore

Answer: (B) and (C) Official key: B;C

  1. Rule: in true centrifugal casting the mould spins about its own axis and the liquid metal is thrown against the mould wall. No core forms the bore. The inner surface is a free surface of the rotating liquid, which sits at constant pressure, so it takes the shape of a paraboloid of revolution, practically a circular cylinder at the 20 to 100 times gravity used.
  2. So the bore must be circular. The outer surface is set by the mould, so it can have any shape that the mould can be made to hold while spinning (a polygonal outline is allowed in the question).
  3. (A) Pentagonal bore: not possible. (B) Circular bore, heptagonal outside: possible. (C) Circular bore, pentagonal outside: possible. (D) Heptagonal bore: not possible, a free liquid surface cannot form a polygon.
  4. The answer is (B) and (C).

Check: if the bore had to be polygonal or off-centre, a core or a semi-centrifugal or centrifuge (pressure) casting method would be needed instead. We tested each option on its bore shape: only a circular bore passes.

Where this shows up in industry

Cast iron pipe, cylinder liners and bushings are made on spinning machines this way, and the bore always comes out round and sound with the lighter slag and inclusions pushed toward the inner surface where they are machined away.

GATE 2026 · PI · Q.45MSQ · 2 marksCasting: solidification, gating, risers and defects

Side riser with d equal to h for a 10 cm steel cube: which diameters can feed the shrinkage

A steel cube of side 10 cm is made by the sand-casting process. A cylindrical side-riser with diameter, , and height, , needs to be used.

Assume:

  • No surface sharing between the riser and casting.
  • .
  • The connecting link between the riser and casting does not freeze before the casting.
  • All the surfaces of the riser and casting are subjected to identical cooling conditions.

In this situation, which ONE or MORE among the following values of d (in cm) can theoretically fully compensate for shrinkage during casting?

  1. (A)5
  2. (B)8
  3. (C)15
  4. (D)20

Answer: (C) and (D) Official key: C;D

  1. Rule (Chvorinov): solidification time with modulus (volume over cooling surface area), and the same here because the cooling conditions are identical. The riser must stay liquid at least as long as the casting, so (practice uses a margin of 1.2). It must also hold enough liquid to feed the shrinkage.
  2. Cube, all six faces cooling: .
  3. Riser with and nothing shared with the casting: volume , area , so cm.
  4. requires cm (and cm with the 1.2 margin). Option moduli: : 0.833; : 1.333; : 2.500; : 3.333 cm. Only 15 and 20 pass, under both the 1.0 and the 1.2 rule.
  5. Volume check with a generous 6% shrinkage of the 1000 cm cube, 60 cm: the 5 cm riser holds 98 cm and passes this test, so volume alone does not eliminate it, but it freezes first and feeds nothing. The answer is (C) and (D).

Trap: a small riser has enough volume to hold the shrinkage but freezes before the casting, so the last liquid has no feed path. Modulus decides, not volume. We tested the cube and each riser with both margins and a volume check: the passing set is (C), (D).

Where this shows up in industry

Foundry engineers size risers by modulus first: the riser must outlast the hot spot it feeds, then they confirm that its volume covers the shrinkage and use insulating or exothermic sleeves to cut the riser size and the yield loss.

GATE 2024 · PI · Q.16MCQ · 1 markMetal forming: rolling, drawing and sheet metal

Match deep drawing cup defects (orange peel, wrinkling, tearing, earing) to their reasons

Match each of the listed defects in deep drawing cup with the corresponding reason in the table.
Defect in deep drawing cupReason
POrange peel on the surface of cup1No blank holding force
QWrinkling at the flange of cup2Very small corner radius of the punch
RTearing at the bottom corner of cup3Large grain size in the blank material
SEarring at the top edge of the cup4Anisotropy of the blank material
  1. (A)P-3, Q-4, R-2, S-1
  2. (B)P-4, Q-1, R-3, S-2
  3. (C)P-3, Q-1, R-2, S-4
  4. (D)P-2, Q-3, R-1, S-4

Answer: (C) Official key: C

  1. In deep drawing a flat blank is pulled by a punch through a die into a cup. The flange metal is squeezed in the hoop direction as it moves inward, and the wall under the punch is stretched. Each defect has a standard cause.
  2. P, orange peel: with large grains each grain deforms on its own and the surface roughens like the skin of an orange. P goes with 3.
  3. Q, wrinkling at the flange: the compressive hoop stress buckles the thin flange unless a blank holder presses it flat, so it comes from no (or too little) blank holding force. Q goes with 1.
  4. R, tearing at the bottom corner: this is the thinnest, most stretched part of the wall. A very small punch corner radius bends the sheet too sharply and splits it. R goes with 2.
  5. S, earing: sheet rolled from a bar has different strength and strain behaviour in different directions (anisotropy), so the cup rim comes out wavy with ears. S goes with 4.
  6. The set is P-3, Q-1, R-2, S-4: (C).

Check: the four options were compared with this cause table in code and only (C) matches. Trap: tying tearing to a missing blank holder (reasons 1 and 2 swapped); too much holding force, not too little, tears a cup, while too little wrinkles it.

Where this shows up in industry

Press shops making cans, kitchen sinks and fuel tanks tune blank-holder force, punch corner radius and lubricant to remove wrinkles and tears, and trim the ears off the cup rim after drawing. Orange peel is controlled by buying sheet with a specified fine grain size.

GATE 2024 · PI · Q.35NAT · 1 markMetal forming: rolling, drawing and sheet metal

Blanking a 100 mm blank from 2 mm sheet with 6% radial clearance: punch diameter in mm

A blank of 100 mm diameter is to be cut out of a 2 mm thick sheet through blanking operation. If the radial clearance between the punch and die is 6% of the sheet thickness then the diameter (in mm) of the punch is __________ . (Rounded off to 2 decimal places)

Answer: 99.76 mm Official key: 99.76 to 99.76

  1. In blanking the punched-out piece is the product, so its size is fixed by the die opening; the clearance is taken off the punch. (In punching a hole it is the other way round: the punch is the size of the hole and the die is larger.)
  2. Radial clearance mm, on each side of the punch.
  3. Die diameter mm. Punch diameter 99.76 mm, equal to the key 99.76 to 99.76.

Check: the clearance acts on both sides of the punch, so the diameter drops by . Slips: taking off only one clearance gives 99.88 mm, and taking 6 % of the diameter gives 94.00 mm; neither is the key.

Where this shows up in industry

Tool makers cut a die to the blank size and grind the punch smaller by twice the clearance, typically 5 to 10 percent of sheet thickness per side. The right clearance controls burr height and the life of the punch and die.

GATE 2024 · PI · Q.39MCQ · 2 marksMetal forming: rolling, drawing and sheet metal

Plane stress 200 and 100 MPa with von Mises yielding: uniaxial tensile yield strength in MPa

In a forming operation, the plastic deformation of a steel specimen starts under plane stress condition, where the principal stresses are MPa and MPa. If the steel specimen follows von-Mises yield criterion, then the uniaxial tensile yield strength (in MPa) of this steel material is _____ (Rounded off to 1 decimal place)
  1. (A)173.2
  2. (B)200.0
  3. (C)100.0
  4. (D)223.6

Answer: (A) Official key: A

  1. A yield criterion tells when a metal starts to flow plastically under combined stresses. The von Mises criterion says yielding starts when the distortion energy equals that at yield in a simple tension test. In terms of the three principal stresses, .
  2. Plane stress means , so .
  3. , so 173.2 MPa: (A).

Check: the other options are the common slips. The Tresca (maximum shear stress) criterion gives the largest of , and , which is 200.0 MPa, option (B). Dropping the cross term gives MPa, option (D). The stress difference, 100.0 MPa, is option (C). The question names von Mises, so only (A) is right, and von Mises is always at or below Tresca here.

Where this shows up in industry

Forming engineers use von Mises equivalent stress to predict when sheet starts to yield in a stamping or deep-drawing simulation. Tresca is a simpler, slightly more conservative choice that is used for quick hand calculations on rolling and extrusion.

GATE 2024 · PI · Q.53NAT · 2 marksMetal forming: rolling, drawing and sheet metal

Cold rolling to 3 mm with 400 mm rolls, bite angle 10 deg, neutral point 7 deg: thickness there in mm

In a single pass cold rolling operation, a flat plate is reduced to a thickness of 3 mm. In this operation, two rolls of diameter 400 mm each are rotating in opposite direction at 300 RPM, and the elastic deflection of these rolls is negligible. The angle of bite is . If the neutral point is present at an angle of from the exit side, then the thickness of the plate (in mm) at the neutral point is __________ . (Rounded off to 1 decimal place)

Answer: 6.0 mm Official key: 5.8 to 6.1

  1. In rolling, the plate is pulled into the gap by friction and the gap between the roll surfaces closes from the entry to the exit. A point on the roll arc is located by its angle measured from the line through the roll centres (the exit plane). The plate thickness there is , where is the exit thickness and the roll radius. (The two rolls each lift the surface by .)
  2. Roll radius mm. The neutral point is where the roll surface speed equals the plate speed; here it is at from the exit side. The roll speed (300 RPM) is not needed for the thickness.
  3. 6.0 mm, inside the key range 5.8 to 6.1.

Check: the small-angle form gives 5.99 mm, so both forms land in the key range. The entry thickness is mm (a draft of 6.08 mm), and the neutral thickness lies between exit and entry as it must. To bite at all, friction must satisfy . Trap: measuring the 7 degrees from the entry side, so that the angle used is 3 degrees, gives 3.55 mm.

Where this shows up in industry

Rolling-mill engineers locate the neutral point to estimate forward slip and the roll torque, and so set the roll speed that keeps strip speed at the exit matched to the coiler. A neutral point that moves toward the exit signals that friction is dropping and the strip is about to slip in the gap.

GATE 2025 · PI · Q.45NAT · 2 marksMetal forming: rolling, drawing and sheet metal

Percentage area reduction in ideal wire drawing with 300 MPa flow stress and 200 MPa front tension

In a wire drawing of a perfectly-plastic material with flow stress of 300 MPa, the back tension is zero and front tension is 200 MPa. Assuming ideal deformation with zero friction, the percentage reduction of the cross-sectional area of the wire is________. (Rounded off to one decimal place)

Answer: 48.7 percent Official key: 47.1 to 49.5

  1. For ideal deformation (no friction, no redundant work) of a perfectly plastic material, the stress in the wire grows only by the work of deformation: with true strain . With back tension the drawing stress at the die exit is .
  2. The front tension is the drawing stress at the die exit, so MPa, and .
  3. , so .
  4. Reduction , that is 48.7 percent, inside the key range 47.1 to 49.5. A step-by-step integration of gave the same value.

Trap: reading 200 MPa as a back tension gives and a reduction of 28.35 percent. The largest reduction this material allows is percent, reached when the drawing stress equals the flow stress.

Where this shows up in industry

Wire mills limit the reduction per die so that the drawing stress stays well below the strength of the wire leaving the die, usually around 20 to 30 percent area reduction per pass. Front tension is the drawing stress, and back tension from a pay-off brake lowers the die pressure and wear.

GATE 2025 · PI · Q.46NAT · 2 marksMetal forming: rolling, drawing and sheet metal

Minimum friction coefficient in cold rolling when the draft is doubled and the rolls are halved in diameter

In a cold rolling process without front and back tensions, the required minimum coefficient of friction is 0.04. Assume large rolls. If the draft is doubled and roll diameters are halved, then the required minimum coefficient of friction is________. (Rounded off to two decimal places)

Answer: 0.08 Official key: 0.08 to 0.08

  1. Rolling can only bite the strip if friction at the roll contact can pull it in. The limit is , where is the angle of contact. For large rolls the draft is , so the minimum friction is .
  2. Draft doubled: . Diameter halved, so .
  3. .
  4. Check without the large-roll shortcut: with the exact new value is 0.0801, which also rounds to 0.08.

Trap: only doubling the draft gives . Both changes act inside the square root, so they multiply by .

Where this shows up in industry

Cold mills need rough or lightly lubricated rolls on the first passes of a heavy reduction, and small work rolls are used for thin strip to cut the roll force. The bite limit tells the mill operator the largest draft a given roll radius and lubricant can take without the strip slipping.

GATE 2026 · PI · Q.26MSQ · 1 markMetal forming: rolling, drawing and sheet metal

Match defects (centerburst, earing, zipper cracks, cold shut) with the processes where they occur

Which ONE or MORE among the following options CORRECTLY match(es) the type of defects with the corresponding metal working processes in which they are likely to occur?
DefectProcess
PCenterburst1Deep drawing
QEaring2Rolling
RZipper cracks3Extrusion
SCold shut4Closed die forging
5Casting
  1. (A)P-3; Q-1; R-2; S-4
  2. (B)P-5; Q-2; R-3; S-4
  3. (C)P-1; Q-2; R-4; S-5
  4. (D)P-3; Q-1; R-2; S-5

Answer: (A) and (D) Official key: A;D

  1. Centerburst (chevron) cracks form inside the billet along the axis in extrusion (and drawing) when the die angle and reduction are too high, so P goes with 3.
  2. Earing is the wavy, ear-like rim of a drawn cup caused by planar anisotropy of the sheet: deep drawing, so Q goes with 1.
  3. Zipper cracks are cracks along the centre of the strip, seen in flat rolling, so R goes with 2.
  4. Cold shut is a seam where two streams of metal meet without fusing. It occurs in casting (two cooled fronts of liquid) and in closed-die forging (a fold of metal pressed into the surface), so S goes with 4 and also with 5.
  5. Option (A) uses S-4 and (D) uses S-5; both are correct. (B) fails on P-5 and (C) fails on P-1. The answer is (A) and (D).

Trap: S has two valid partners, so two options can be right together. We stored for each defect the set of processes where it occurs and tested every option: (A) and (D) pass, (B) and (C) fail on P.

Where this shows up in industry

Press-shop and forge quality teams use these names as inspection codes: ears on a drawn cup are trimmed and tracked to sheet anisotropy, centre bursts are found by ultrasonic testing of extruded bar, and cold shuts show up as surface seams in forgings and castings.

GATE 2026 · PI · Q.30NAT · 1 markMetal forming: rolling, drawing and sheet metal

Minimum blanking force for a 50 mm square cut from 2 mm strip with 200 MPa shear strength

A square of side length 50 mm is to be blanked from a strip of 2 mm thickness. The sheet metal has a shear strength of 200 MPa.

To enable a single step blanking operation, the theoretical minimum blanking force required is ______ N (in integer).

Note: Neglect the effect of clearances and friction.

Answer: 80 Official key: 80 to 80

  1. Rule: blanking shears the metal all round the cut edge, so the force is the shear strength times the sheared area: . With no clearance or friction this is the theoretical minimum.
  2. Perimeter of the square . Sheared area .
  3. , so the answer is 80.

Trap: using the plan area instead of the sheared edge area gives a nonsense 500 kN. The metal is cut along the edge, not across the face. We recomputed from perimeter, thickness and shear strength.

Where this shows up in industry

Press tonnage for a blanking die is estimated this way before choosing the press, and a shear (angled) face on the punch is added to cut the peak force when the press is close to its rating.

GATE 2026 · PI · Q.39MCQ · 2 marksMetal forming: rolling, drawing and sheet metal

Feasible blank diameter for deep drawing with 2 mm sheet and a 100 mm punch

A sheet metal drawing is considered feasible if the following conditions are met:
  • Reduction ratio
  • Thickness to diameter ratio

A sheet metal drawing process is being planned on a sheet metal with a thickness of 2 mm with a punch of diameter 100 mm with various blanks of diameter .

Which ONE of the following blank diameters (in mm) will result in feasible drawing?

  1. (A)150
  2. (B)250
  3. (C)350
  4. (D)450

Answer: (A) Official key: A

  1. Rule: the reduction ratio in drawing is (the same as a limiting drawing ratio ). The thickness ratio is . Both limits must hold: a wide blank makes drawing too severe and a thin blank wrinkles.
  2. Reduction ratio means , so .
  3. Thickness ratio means , so as well.
  4. Check the options: 150 mm gives and , both pass. 250 mm gives and , both fail; 350 mm and 450 mm fail more. The answer is (A) 150.

Trap: the two conditions give the same limit here, so they do not need separate treatment, but a reduction ratio defined as (not ) would flip the inequality. We tested every blank against both conditions: only 150 mm passes.

Where this shows up in industry

Cup-drawing process planning starts with a limiting drawing ratio of about 2 for steel and aluminium. Beyond it the cup tears at the punch radius, so a deeper part is drawn in two or more stages with intermediate anneals.

GATE 2026 · PI · Q.46MSQ · 2 marksMetal forming: rolling, drawing and sheet metal

Rolling 23 mm strip to 20 mm in one pass: which lubricants give enough friction to bite

In a rolling operation, a 200 mm wide strip of 23 mm thickness needs to be reduced to 20 mm in a single pass. The roll diameter is 200 mm. Four lubricants P, Q, R, and S with coefficient of friction 0.05, 0.1, 0.2, and 0.25, respectively, are available for use at the roll-strip interface. Assume that the strip width remains constant throughout the process.

Which ONE or MORE among the following lubricants will enable the rolling process to achieve the desired final thickness of the strip in a single pass?

  1. (A)P
  2. (B)Q
  3. (C)R
  4. (D)S

Answer: (C) and (D) Official key: C;D

  1. Rule: the rolls can only pull the strip in (bite) if friction is high enough. Bite needs with contact angle , and the largest draft possible in one pass is .
  2. Required draft and . So , giving . The exact bite angle () gives , the same set of lubricants.
  3. Maximum draft per lubricant: P (0.05) mm; Q (0.1) mm; R (0.2) mm; S (0.25) mm. Only R and S reach 3 mm.
  4. The answer is (C) and (D).

Trap: a better lubricant (lower ) is normally preferred in service because it lowers the roll force, but here a reduction of 3 mm needs a minimum friction to pull the strip in. The best lubricant (P) fails. Both the draft formula and the exact bite angle agree on the passing set.

Where this shows up in industry

Mill operators meet this limit when the first pass of a thick slab or a plate must bite: they roughen or sand the rolls, or use a lightly lubricated first pass and a smaller draft, then use heavy lubrication on later, thinner passes.

GATE 2024 · PI · Q.29MSQ · 1 markJoining: welding, brazing and friction stir welding

Friction stir welding: which statements are true (joint types, melting, retreating and advancing side)?

Which among the following is/are TRUE for friction stir welding (FSW) process?
  1. (A)It can be used to produce lap, butt and tee joints.
  2. (B)A non-consumable rotating tool with shoulder and pin is used to melt the work-piece material.
  3. (C)Retreating side of the weld is where the linear velocity vector at a point on that side of the rotating tool and the welding direction are opposite.
  4. (D)Advancing side of the weld is where the linear velocity vector at a point on that side of the rotating tool and the welding direction are opposite.

Answer: (A) and (C) Official key: A;C

  1. Friction stir welding pushes a spinning, non-consumable tool, a pin with a wider shoulder, into the seam and travels along it. Friction and stirring soften the metal so that it flows around the pin and fuses in the solid state. Think of it as kneading two pieces of hot dough together.
  2. (A) True. The tool only needs access to the seam, so butt, lap, tee and corner joints are all made.
  3. (B) False. The tool is non-consumable and rotating, but it does not melt the work-piece: the metal stays below its melting point, which is why FSW avoids solidification cracks and porosity.
  4. (C) True. Each point on the tool surface has a tangential velocity from the rotation. On the retreating side that velocity points against the welding (travel) direction, so the relative speed between tool and metal is lower there.
  5. (D) False. On the advancing side the tangential velocity points along the welding direction (the relative speed is the sum of rotation and travel speeds). Statement D describes the retreating side. Hence (A) and (C).

Check: for a tool travelling along , the rotational velocity at a point is . Seen from above, a clockwise tool makes the left-hand side of the travel direction advancing and the right-hand side retreating, and an anticlockwise tool the reverse; the vector test confirmed both cases. Trap: marking D as true because the two side names are easy to swap.

Where this shows up in industry

FSW is used for aluminium fuel tanks, rail-car panels, battery trays and ship decks, where a melt-free weld keeps strength and avoids distortion. Weld engineers also choose the tool rotation direction so that the better-quality advancing side faces the critical edge.

GATE 2024 · PI · Q.52NAT · 2 marksJoining: welding, brazing and friction stir welding

Two arc welds with equal heat input: 180 A at 6 mm/s, find the current at 8 mm/s (30 V, 85% efficiency)

Mild steel plates are welded to make butt joints by arc welding with 85% heat transfer efficiency ignoring other losses. The first weld joint is made by selecting arc voltage of 30 V and current of 180 A with a welding speed of 6 mm/s. Using identical plates, a second weld joint is made with the same arc voltage and a welding speed of 8 mm/s. If both the welds have the same heat input, then the welding current (in A) for the second weld joint is __________ . (Answer in integer)

Answer: 240 A Official key: 240 to 240

  1. Heat input of an arc weld is the heat that enters the work per millimetre of weld: , with efficiency , arc voltage , current and travel speed . A faster torch spreads the same arc power over more length, so the heat per millimetre falls.
  2. Weld 1: J/mm (0.77 kJ/mm).
  3. Weld 2 has the same and and must have the same , so .
  4. 240 A, equal to the key 240 to 240.

Check: the efficiency and the voltage are the same on both sides, so they cancel and current is proportional to speed. Trap: scaling current with the inverse of speed (135 A), which would lower the heat input.

Where this shows up in industry

Welding procedure specifications fix heat input in kJ per mm for each steel grade, because too high a value coarsens the heat-affected zone and too low a value risks cracking. When a welder raises the travel speed, the current is raised in proportion to hold the same heat input.

GATE 2025 · PI · Q.16MCQ · 1 markJoining: welding, brazing and friction stir welding

Welding process in which an exit hole is common

Exit-hole occurrence is common in
  1. (A)Electron Beam Welding
  2. (B)Submerged Arc Welding
  3. (C)Friction Welding
  4. (D)Friction Stir Welding

Answer: (D) Official key: D

  1. An exit hole is a hole left at the end of a seam where the welding tool or beam was pulled out.
  2. In friction stir welding a rotating tool with a pin is plunged into the joint line and travelled along it. The pin is longer than a point, so when the tool is withdrawn at the end of the seam it leaves a pin-shaped hole. This is the exit (keyhole) hole. It is removed by running onto a tab, filled by a repair plug, or avoided with a retractable pin tool.
  3. (A) Electron beam welding does melt a vapour keyhole, but it closes behind the beam and the weld ends in a small crater. (B) Submerged arc welding ends in a crater, handled by a run-off tab. (C) Friction welding joins two parts by rotation and upset and leaves flash, with no pin to withdraw.
  4. So the process with a characteristic exit hole is (D).

Trap: the electron beam keyhole is real, but it is a transient cavity during welding, not a tool-shaped hole left in the part.

Where this shows up in industry

Friction stir welded aluminium tanks, rail car panels and battery trays are finished with the exit hole on a run-off tab or closed with a friction plug weld. Retractable-pin tools are used where the hole cannot be tolerated.

GATE 2025 · PI · Q.47NAT · 2 marksJoining: welding, brazing and friction stir welding

Maximum arc length in DC arc welding with V = 30 + 30 l and 80 V open circuit voltage

In a direct current arc welding, the voltage V (in volt) is related to the arc length l (in cm) as . The open circuit voltage is 80 volts. The maximum possible arc length (in cm) is________. (Rounded off to two decimal places)

Answer: 1.67 cm Official key: 1.65 to 1.69

  1. A power source delivers current only while the arc voltage is below its open circuit voltage. The source line is , so the current is positive only if . At the current is zero and the arc cannot be kept alive.
  2. The longest arc that can still be sustained is therefore the one whose arc voltage just equals 80 V: .
  3. cm, which is 1.67 cm to two decimals. Scanning the arc length against the source line for three different short-circuit currents gave the same limit.

Trap: the 40 V point (half the open circuit voltage) is the maximum power condition and gives cm. The question asks for the longest possible arc, not the most powerful one. The paper prints the symbol in a typeface that looks like the digit 1, so the equation appears as 30 + 301.

Where this shows up in industry

Welders see this as the arc stretching and going out when the electrode is lifted too far from the work. Manual arc sets use a drooping characteristic so that small changes in arc length change the current only a little.

GATE 2026 · PI · Q.12MCQ · 1 markJoining: welding, brazing and friction stir welding

Which statement about the filler material in brazing is FALSE

Which ONE of the following is FALSE with respect to filler material used in brazing?
  1. (A)Melting temperature of the filler material must be less than the base metal.
  2. (B)Wettability of the base metal by the filler material must be low.
  3. (C)Viscosity of the filler material must be low for penetration into the interface.
  4. (D)Chemical reactivity between the filler material and the base metal must be low.

Answer: (B) Official key: B

  1. Rule: in brazing the filler metal melts and is drawn into a tight joint gap by capillary action; the base metal stays solid. The filler therefore needs a lower melting point than the base metal, good wetting, low viscosity and low reactivity.
  2. (A) True. The filler melts above 450 °C but below the base metal, so the parts never melt.
  3. (B) False. Wetting means the liquid spreads over the solid surface (small contact angle). Capillary flow and a strong bond need wettability to be HIGH. A filler that wets poorly beads up like water on wax and leaves the gap empty.
  4. (C) True. A thin, runny liquid is drawn into gaps of about 0.05 to 0.25 mm.
  5. (D) True. Little reaction avoids brittle intermetallic layers and erosion of the base metal. Only (B) is false, so the answer is (B).

Trap: the word 'low' appears in three options. Read each for the property, not the adjective: low viscosity and low reactivity help, low wettability does not. We encoded each statement as true or false with its reason: the false set is only (B).

Where this shows up in industry

Brazing of copper tube joints in refrigeration coils and of carbide tips onto tool shanks depends on choosing a filler that wets the surfaces and flows into a gap of a fraction of a millimetre, which is why flux or a controlled atmosphere is used to keep the surfaces wettable.

GATE 2026 · PI · Q.13MCQ · 1 markJoining: welding, brazing and friction stir welding

Arc welding speed from a 6 kW source with 50% loss, 10 mm2 weld and 15 J/mm3 melting energy

An arc welding process is being carried out with a power source of 6 kW to weld two similar metals. The total energy loss is 50%, the area of cross-section of the weld is 10 mm2, and the specific energy needed to melt the metal is 15 J/mm3.

The speed of welding is ______ mm/s.

  1. (A)10
  2. (B)20
  3. (C)30
  4. (D)40

Answer: (B) Official key: B

  1. Rule (energy balance): the power that reaches the work, source power (1 minus loss), must supply the energy to melt the metal laid down each second. Melting rate (cross-section speed), so with the specific melting energy.
  2. Useful power .
  3. Volume melted per second .
  4. Speed , so the answer is (B).

Trap: forgetting the 50% loss gives , option (D). We tested every option: only 20 mm/s makes equal to the 3000 W that reaches the work.

Where this shows up in industry

Weld procedure sheets are built on this balance: for a given arc power and joint cross-section, the travel speed is limited by how fast the metal can be melted, and welders and robots are programmed to a speed window around it.

GATE 2024 · PI · Q.38MCQ · 2 marksPowder metallurgy, polymers and composites

Polymers: match extrusion, injection, blow and compression moulding with their applications

For polymers, match each process with the most suitable application listed.
ProcessApplication
PExtrusion1Producing complex parts with close tolerance
QInjection molding2Producing thermosetting plastic components
RBlow molding3Producing long uniform sections
SCompression molding4Producing hollow shapes
  1. (A)P-3, Q-1, R-2, S-4
  2. (B)P-2, Q-3, R-4, S-1
  3. (C)P-4, Q-2, R-1, S-3
  4. (D)P-3, Q-1, R-4, S-2

Answer: (D) Official key: D

  1. Match each process by what it can and cannot make.
  2. P, extrusion: a screw pushes melt continuously through a die, and the profile stays the same along its length, so it makes long uniform sections (pipes, rods, sheet). P goes with 3.
  3. Q, injection moulding: melt is injected at high pressure into a closed steel cavity, which copies detail and size very accurately, so it makes complex parts with close tolerance. Q goes with 1.
  4. R, blow moulding: a hot tube of plastic is inflated like a balloon against a mould wall, so it makes hollow shapes such as bottles. R goes with 4.
  5. S, compression moulding: a charge is pressed and heated in an open mould until it cures, the classic route for thermosetting plastic components (they set permanently and cannot be re-melted). S goes with 2.
  6. The set is P-3, Q-1, R-4, S-2: (D).

Check: all four options were compared with these pairs in code and only (D) matches. Trap: giving thermosets to injection moulding; most injection moulding is of thermoplastics, and thermosets are the textbook case for compression moulding.

Where this shows up in industry

Plastic pipes and window profiles are extruded, phone cases and gears are injection moulded, water bottles and fuel tanks are blow moulded, and electrical switch housings and brake pads are compression moulded from thermoset charges.

GATE 2025 · PI · Q.21MCQ · 1 markPowder metallurgy, polymers and composites

FALSE statement about injection moulding of a polymer composite

Which one of the following statements is FALSE with respect to the injection molding of polymer composite?
  1. (A)Molten polymer along with the reinforcements is injected into a closed mold cavity.
  2. (B)Material deforms plastically to adopt the shape of the mold cavity.
  3. (C)Melt temperature, injection speed and screw speed are some important process parameters.
  4. (D)Commonly used reinforcements are particles, whiskers and short fibers.

Answer: (B) Official key: B

  1. In injection moulding a screw melts the polymer and mixes in the reinforcement, then pushes the melt at high pressure through a nozzle and runner into a closed, cooled mould. The part is ejected once it has solidified.
  2. (A) True. This is the basic process description.
  3. (C) True. Melt temperature, injection speed, screw speed, holding pressure and mould temperature control filling and part quality.
  4. (D) True. Short fibres, whiskers and particles can be carried in the melt without blocking the gate. Continuous fibres cannot be injected, so they are not used.
  5. (B) False. The material takes the cavity shape because it is a liquid melt that flows into it, not because a solid deforms plastically as in forging or sheet forming. The shape is then frozen by cooling.

Check: the false statement is the only one that describes the material as a solid being plastically deformed.

Where this shows up in industry

Glass-filled nylon and polypropylene housings, gears and automotive brackets are made this way, with the fibre content kept short so the melt still fills the cavity. Moulders watch melt temperature and screw speed because they change fibre length and warpage.

GATE 2026 · PI · Q.36MCQ · 2 marksPowder metallurgy, polymers and composites

Match extruded round and square polymer cross-sections with the die opening that most likely made them

In a polymer extrusion process, some cross-sectional shapes of the extruded polymers are shown. Cross-sections of available dies are also shown.

Which ONE of the following CORRECTLY matches the extruded cross section with the die opening that most likely generated it?

Note: The cross-sections are in a plane orthogonal to the extrusion direction. Figures are not to scale.

Polymer extrusion. Top: two extruded cross-sections, (P) a round bar and (Q) a square bar. Bottom: four die openings, each a round die plate with a hole: (1) small round hole, (2) square hole, (3) elliptical hole, (4) a square hole with concave, inward-curved sides. Figures are not to scale.Cross-section of extruded polymerCross-section of die opening(P)(Q)(1)(2)(3)(4)
  1. (A)P-1; Q-4
  2. (B)P-1; Q-2
  3. (C)P-3; Q-2
  4. (D)P-3; Q-4

Answer: (A) Official key: A

  1. Rule: die swell (extrudate swell). A polymer melt is elastic. After it leaves the die the stored elastic strain relaxes, so the extrudate is larger than the opening and sharp features are rounded off.
  2. Round bar P: only a round die opening is round after swell, because swell acts equally in every direction. We computed the rotational symmetry of each outline: the round hole (1) repeats under every rotation, the square (2) and the concave square (4) under 90 degrees, the ellipse (3) only under 180 degrees. An elliptical hole stays elliptical, so P-3 is out and P goes with 1.
  3. Square bar Q: a straight-sided square hole (2) swells into a rounded, bulging section: the corners round and the sides bow out. To get flat sides, the die must be the other way, with inward-curved (concave) sides that the swell fills out. Of the two dies with 90-degree symmetry, (2) and (4), only (4) has the compensating sag, so Q goes with 4.
  4. The answer is (A) P-1; Q-4.

Trap: matching the shape to the shape (square bar from square hole, option B) ignores swell. The true die is often not the shape of the product.

Where this shows up in industry

Profile extrusion dies for window frames, trims and tubing are cut to a pre-compensated shape, then trimmed and re-cut after trials because the swell depends on the polymer grade, melt temperature and line speed.

GATE 2026 · PI · Q.37MCQ · 2 marksPowder metallurgy, polymers and composites

Degree of densification of gas-atomised iron powder from tap, apparent and solid densities

Iron powder produced by gas atomization has a tap density and an apparent density of 3.26 g/cm3 and 2.66 g/cm3, respectively. The density of solid iron is 7.85 g/cm3.

Which ONE of the following options is the closest approximation to the degree of densification (in percentage) of this iron powder?

  1. (A)41.52
  2. (B)81.59
  3. (C)33.89
  4. (D)75.41

Answer: (C) Official key: C

  1. Terms: apparent density is the mass of loose powder poured into a container divided by the container volume (powder not yet disturbed). Tap density is the same after tapping, which packs the grains closer. The solid (theoretical) density is that of fully dense iron. A density ratio to solid is a fraction of the volume that is metal.
  2. The official key is (C), , that is 33.89%: the fraction of the volume the poured, undensified powder fills. Taking the question's 'degree of densification' as the density of the powder as it is, relative to solid iron, this is the apparent density divided by the solid density.
  3. We enumerated every sensible ratio of the three densities against the four options. Tap over solid, , gives , which is option (A); apparent over tap, , gives , option (B); the sum of tap and apparent over solid gives , option (D), which has no physical meaning. The keyed value (C) is reproduced only by apparent over solid.
  4. So the answer is (C) 33.89.

Honest note: many texts would call tap density over solid density the packing level reached after tapping, which is 41.5%, option (A). The question is ambiguous, and the official key follows the apparent-density reading. For GATE, remember this key. A true measure of tapping-induced densification would be , which is not offered.

Where this shows up in industry

Powder suppliers report apparent density, tap density and flow rate on every lot of iron powder, because the loose fill density sets how deep the die must be filled and how much the powder must shrink under the punch to reach the target density.

GATE 2026 · PI · Q.65NAT · 2 marksPowder metallurgy, polymers and composites

Axial slider velocity in filament winding of a 700 mm mandrel at 6 rpm for a 45 degree helix

In the composite filament winding process as shown in the figure, the mandrel diameter is 700 mm and is rotating at a speed, rev/min.

If a 45° helical winding angle is needed, the axial velocity, , of the slider should be ______ m/s (rounded off to two decimal places).

Assume . Ignore the thickness of the composite layers already wound on the mandrel.

Filament winding. A cylindrical mandrel with a capsule outline lies horizontally and rotates at N about its axis (curved arrow at the right). A slider above it carries the fibre and moves to the right at axial velocity vc. The fibre lays down helical turns on the mandrel at a helix angle of 45 degrees measured from the mandrel axis. Not to scale.slidervc45°MandrelN

Answer: 0.22 m/s Official key: 0.21 to 0.23

  1. Rule: the fibre leaves the slider and is laid on the mandrel surface. The surface moves round at while the slider moves along the axis at . The fibre direction is the resultant of the two, so with the helix angle measured from the axis, .
  2. Surface speed: , so .
  3. , so the answer is 0.22 m/s.

Check: at exactly 45 degrees the tangent is 1, so measuring the angle from the axis or from the hoop (circumferential) direction gives the same speed (the other reading is ), and exact gives 0.2199 m/s, the same to two decimals. We computed both readings and both values of : all land in 0.21 to 0.23.

Where this shows up in industry

Winding machines for pressure vessels, drive shafts and pipes are programmed from this relation: the carriage speed is tied to the mandrel speed so that the fibre lies at the designed angle, and a 45 degree wind is used where torsion loading needs shear stiffness.

From GATE prep to a production, foundry, press shop or welding career

Talk to a counsellor.

Talk to a career counsellor

Free 20-minute call. We'll map the right course to where you want to work.

By submitting you agree to our Terms and Privacy Policy.

Talk to a career counsellor

Talk to a career counsellor

Free 20-minute call. We'll map the right course to where you want to work.

By submitting you agree to our Terms and Privacy Policy.