GATE Mechanical: Engineering Materials, Casting, Forming and Joining, previous-year questions solved

Real manufacturing questions from the last four GATE Mechanical papers: phase diagrams and heat treatment, casting (Chvorinov's rule, risers, shrinkage, defects), metal forming (rolling, extrusion, wire drawing, blanking, deep drawing) and welding (arc characteristics, heat input, filler feed). Each one has a step-by-step solution that matches the official answer key, and a note on where the idea shows up on the shop floor: foundries, press shops, rolling mills and body-in-white welding lines.

Questions from official GATE ME papers (IIT Kharagpur 2022, IISc Bengaluru 2024, IIT Roorkee 2025, IIT Guwahati 2026); solutions by Skill-Lync. · Updated 16 Nov 2026 · 25 questions

GATE 2022 · ME Set-1 · Q.41MCQ · 2 marksEngineering materials and heat treatment

A 0.5% carbon steel is slowly cooled. What fraction is pro-eutectoid ferrite?

In Fe-Fe3C phase diagram, the eutectoid composition is 0.8 weight % of carbon at 725 ºC. The maximum solubility of carbon in α-ferrite phase is 0.025 weight % of carbon. A steel sample, having no other alloying element except 0.5 weight % of carbon, is slowly cooled from 1000 ºC to room temperature. The fraction of pro-eutectoid α-ferrite in the above steel sample at room temperature is
  1. (A)0.387
  2. (B)0.864
  3. (C)0.475
  4. (D)0.775

Answer: (A) Official key: A

  1. Pro-eutectoid ferrite forms above 725 ºC, before any pearlite. Its amount is fixed just below the eutectoid line, where the steel is ferrite (0.025% C) plus pearlite (0.8% C).
  2. Lever rule on that tie line: : option (A).

Option (D), 0.775, is the denominator of the lever rule, and (B) is the total ferrite counted on the full room-temperature tie line to cementite. The question asks only for the pro-eutectoid part.

Where this shows up in industry

The ferrite-to-pearlite split sets the strength and machinability of plain carbon steels. A 0.45-0.5% C steel such as C45 or EN8, used for shafts, axles and gears, is roughly 40-45% ferrite and the rest pearlite when normalised, which is why it machines well and still takes induction hardening.

GATE 2022 · ME Set-1 · Q.27MSQ · 1 markEngineering materials and heat treatment

Which heat treatments are used for surface hardening of steels?

Which of the following heat treatment processes is/are used for surface hardening of steels?
  1. (A)Carburizing
  2. (B)Cyaniding
  3. (C)Annealing
  4. (D)Carbonitriding

Answer: (A, B, D) Official key: A, B, D

  1. Carburizing adds carbon to the surface, cyaniding adds carbon and nitrogen from a molten cyanide bath, and carbonitriding adds both from a gas atmosphere. Each is followed by quenching, so a hard case forms over a tough core.
  2. Annealing heats the whole part and cools it slowly to soften it and relieve stresses: it hardens nothing.

Answer: (A), (B) and (D).

Where this shows up in industry

Gearbox gears, camshafts and bearing races are case hardened: a hard, wear-resistant skin over a tough core that survives shock loads. Carburizing is the workhorse for transmission gears; cyaniding is now rare because the cyanide salts are toxic to handle and dispose of.

GATE 2024 · ME · Q.28MCQ · 1 markEngineering materials and heat treatment

Which two phases make up pearlite?

The phases present in pearlite are
  1. (A)austenite and ferrite
  2. (B)cementite and austenite
  3. (C)ferrite and cementite
  4. (D)martensite and ferrite

Answer: (C) Official key: C

  1. Pearlite forms when austenite of eutectoid composition (about 0.8% C) cools slowly through the eutectoid temperature.
  2. It transforms into alternating thin plates (lamellae) of ferrite (almost pure iron) and cementite (Fe3C): option (C).

Pearlite is a microconstituent, not a phase: it contains two phases. Austenite is gone after the transformation, and martensite forms only on fast quenching.

Where this shows up in industry

Rail steel is almost fully pearlitic: the fine ferrite-cementite plates give high wear resistance under wheel contact. Rail makers head-harden rails by cooling them faster, which makes the pearlite spacing finer and the rail harder.

GATE 2025 · ME · Q.20MCQ · 1 markEngineering materials and heat treatment

Which surface hardening process heats steel to the lowest temperature?

Among the following surface hardening processes, steel is heated to the lowest temperature in
  1. (A)carburizing
  2. (B)cyaniding
  3. (C)nitriding
  4. (D)carbonitriding

Answer: (C) Official key: C

  1. Carburizing, cyaniding and carbonitriding all need the steel to be austenite so carbon can dissolve and diffuse, which means heating above about 800 ºC (carburizing typically 900-950 ºC).
  2. Nitriding diffuses nitrogen into ferritic steel at about 500-550 ºC, below the lower critical temperature, and needs no quench: option (C).
Where this shows up in industry

Because nitriding stays below the transformation temperature and has no quench, parts barely distort. That is why finish-machined crankshafts, plastic-injection screws and die-casting dies are nitrided after machining rather than carburized.

GATE 2026 · ME · Q.62NAT · 2 marksEngineering materials and heat treatment

An FCC metal has density 2.71 g/cm³ and atomic weight 26.98 g/mol. What is its atomic radius?

A metal has FCC crystal structure with 2.71 g/cm3 of density and 26.98 g/mol of atomic weight. The Avogadro’s number is . The atomic radius of the metal is ________ nm (rounded off to 2 decimal places).

Answer: 0.14 nm Official key: 0.12 to 0.16

  1. An FCC unit cell holds 4 atoms ().
  2. Density , so , giving .
  3. In FCC the atoms touch along the face diagonal: , so .

Using the BCC contact () by mistake gives 0.175 nm. The metal is aluminium, whose handbook atomic radius is 0.143 nm.

Where this shows up in industry

Lattice parameter and atomic radius are what X-ray diffraction measures. Labs use the shift in an aluminium alloy's lattice parameter to estimate how much magnesium or copper is in solid solution, and to measure residual stress in machined and welded parts.

GATE 2022 · ME Set-2 · Q.19MCQ · 1 markCasting

A 15% B alloy is poured at 800 °C. What is its solidification range on this phase diagram?

Fluidity of a molten alloy during sand casting depends on its solidification range. The phase diagram of a hypothetical binary alloy of components A and B is shown in the figure with its eutectic composition and temperature. All the lines in this phase diagram, including the solidus and liquidus lines, are straight lines. If this binary alloy with 15 weight % of B is poured into a mould at a pouring temperature of 800 ºC, then the solidification range is
Hypothetical A-B binary phase diagram with straight lines: melting point of A 700 degrees C; liquidus falls to the eutectic at 30 weight percent B and 400 degrees C; alpha solidus falls from 700 degrees C to 10 percent B at 400 degrees C; the 15 percent B alloy is poured at 800 degrees C04007008000101530Composition (weight % of B in A)Temperature (°C)Lα+Lαβ+LβEutectic point(30%, 400 °C)poured at 800 °CL: liquidα: A-rich solidβ: B-rich solid
  1. (A)400 ºC
  2. (B)250 ºC
  3. (C)800 ºC
  4. (D)150 ºC

Answer: (D) Official key: D

  1. Solidification starts where the 15% line meets the liquidus. The liquidus runs straight from (0%, 700 ºC) to the eutectic (30%, 400 ºC), so .
  2. Solidification ends on the solidus. The α solidus reaches 400 ºC at 10% B; at 15% B the alloy lies past it, so the last liquid freezes as eutectic at 400 ºC.
  3. Range : option (D).

The pouring temperature is a distractor: (option A) counts the superheat, which is lost while the metal is still fully liquid.

Where this shows up in industry

Foundries pick near-eutectic alloys for thin-walled castings because a short freezing range means the metal stays fluid and fills the mould. That is why most die-cast aluminium parts, such as gearbox housings and engine brackets, use high-silicon Al-Si alloys such as ADC12 (about 10-12% Si) or A413 (about 12% Si), near the 12.6% Si eutectic.

GATE 2022 · ME Set-2 · Q.27MSQ · 1 markCasting

A cylindrical riser with an insulated top feeds a cube casting. Which riser radii are acceptable?

Consider sand casting of a cube of edge length . A cylindrical riser is placed at the top of the casting. Assume solidification time, , where is the volume and is the total surface area dissipating heat. If the top of the riser is insulated, which of the following radius/radii of riser is/are acceptable?
  1. (A)
  2. (B)
  3. (C)
  4. (D)

Answer: (A, B), or (B) alone Official key: A, B OR B

  1. The riser must freeze after the casting, so its modulus must be at least the casting's.
  2. Cube: .
  3. Riser of radius and height : the top is insulated and the bottom sits on the casting, so only the side wall loses heat. , whatever the height.
  4. gives , so and are acceptable; and freeze first and cannot feed.

The official key also accepts (B) alone. At the riser modulus only equals the cube's, and if you also remove the patch under the riser from the cube's cooling area, the cube's modulus is larger than and only is safe. Both readings were checked.

Where this shows up in industry

Foundries usually size risers about 20% above the casting's modulus (the 1.2 factor from Wlodawer's method is a common rule), and use insulating or exothermic sleeves to raise the riser's effective modulus. A sleeved riser can be smaller, which saves metal that would otherwise be cut off and remelted.

GATE 2024 · ME · Q.31MCQ · 1 markCasting

Which pattern allowance is provided for easy withdrawal from a sand mould?

The allowance provided to a pattern for easy withdrawal from a sand mold is
  1. (A)finishing allowance
  2. (B)shrinkage allowance
  3. (C)distortion allowance
  4. (D)shake allowance

Answer: (D) Official key: D

  1. Before the pattern is lifted out, the moulder raps (shakes) it so it comes loose from the sand. Rapping enlarges the cavity slightly.
  2. The shake (rapping) allowance makes the pattern a little smaller to cancel that enlargement. It is the allowance tied to withdrawing the pattern: option (D).

Shrinkage allowance compensates for the metal contracting, finishing allowance leaves stock for machining, and distortion allowance pre-bends shapes that warp as they cool. Draft (taper) also helps withdrawal, but it is not among the options.

Where this shows up in industry

Shake allowance is a hand-moulding idea. On automated moulding lines the pattern plate is withdrawn mechanically without rapping, so draft angles of about 1-3° on vertical faces do the job instead.

GATE 2024 · ME · Q.61NAT · 2 marksCasting

A 20 mm cube and a 20 mm diameter sphere are cast in the same mould material. What is the ratio of their solidification times?

Aluminium is casted in a cube-shaped mold having dimensions as 20 mm × 20 mm × 20 mm. Another mold of the same mold material is used to cast a sphere of aluminium having a diameter of 20 mm. The pouring temperature for both cases is the same. The ratio of the solidification times of the cube-shaped mold to the spherical mold is ________ (answer in integer).

Answer: 1 Official key: 1 to 1

  1. Chvorinov's rule: , and is the same for both (same metal, mould material and pouring temperature).
  2. Cube: .
  3. Sphere: .
  4. Equal moduli, so the ratio is .

The cube holds about twice the metal of the sphere (8,000 vs 4,189 mm3), but it also has about twice the cooling area, so both freeze in the same time.

Where this shows up in industry

Casting simulation software computes this modulus for every region of a part to find hot spots, the thick sections that freeze last and shrink. Methoding engineers then place risers or chills at those spots before cutting any tooling.

GATE 2025 · ME · Q.34NAT · 1 markCasting

A 200 mm cube cavity, 7% solidification shrinkage and 8% solid contraction. What is the final edge?

A liquid metal is poured in a mold cavity of size 200 mm × 200 mm × 200 mm. The cooling is uniform in all directions with NO additional compensation for shrinkage. Considering the volumetric shrinkage during solidification and solid contraction as 7% and 8%, respectively, the length of the cube edge after cooling down to the room temperature is _______ mm (rounded off to 1 decimal place).

Answer: 189.9 mm Official key: 189.8 to 190.0

  1. The two shrinkages act one after the other, so they multiply: .
  2. Uniform cooling keeps the cube shape: edge .

Adding the percentages (15%) gives 189.5 mm, which is outside the key range.

Where this shows up in industry

In a real casting, risers feed the solidification shrinkage, and only the solid contraction is built into the pattern as a shrinkage allowance: about 1% linear for grey iron and 1.3% for aluminium in common pattern tables. Pattern makers once used contraction rules, scales stretched by that percentage.

GATE 2025 · ME · Q.38MCQ · 2 marksCasting

Match the mould elements (riser, chill, skim bob, core, sleeve, inoculant) with their functions.

Match the mold elements in the casting process with the most suitable function
  • P. Blind riser · Q. Chill · R. Skim bob · S. Core · T. Insulating sleeve · U. Inoculant
  • I. Casting with internal cavity · II. Molten metal reservoir · III. Nucleating agent · IV. Assisting in faster heat removal from melt · V. Removal of impurities · VI. Increasing the solidification time
  1. (A)P-II, Q-IV, R-V, S-I, T-VI, U-III
  2. (B)P-II, Q-V, R-VI, S-I, T-III, U-IV
  3. (C)P-V, Q-I, R-VI, S-III, T-II, U-IV
  4. (D)P-II, Q-IV, R-I, S-V, T-VI, U-III

Answer: (A) Official key: A

  1. Blind riser: a closed reservoir of molten metal that feeds shrinkage (II).
  2. Chill: a metal insert in the mould that pulls heat out fast (IV).
  3. Skim bob: a trap in the gating system that catches slag and dross (V).
  4. Core: a sand insert that forms an internal cavity (I).
  5. Insulating sleeve: slows the riser's cooling so it freezes last (VI).
  6. Inoculant: added to the melt to create nucleation sites, for example ferrosilicon in grey iron (III).

Only option (A) has all six. A fast check: only (A) and (D) give Q-IV, and (D) wrongly calls the skim bob a core.

Where this shows up in industry

These six items are the methoding toolkit of every foundry. A cylinder block, for example, uses sand cores for the water jacket and bores, chills at the bearing bulkheads, and inoculation of the iron just before pouring to avoid hard chilled edges.

GATE 2025 · ME · Q.62NAT · 2 marksCasting

A cube and a cylinder (D = H) of the same volume are cast. What is the ratio of their solidification times?

Two metal parts (a cylinder and a cube) of same volume are cast under identical conditions. The diameter of the cylinder is equal to its height. The ratio of the solidification time of the cube to that of the cylinder is________ (rounded off to 2 decimal places).
Assume that solidification time follows Chvorinov’s rule with an exponent of 2.

Answer: 0.85 Official key: 0.83 to 0.87

  1. Cube of edge : . Cylinder with : .
  2. Same volume: , so .
  3. .

The cylinder freezes later because it is the more compact shape. A sphere would be slower still, which is why risers are made as compact as possible.

Where this shows up in industry

This is why most risers are cylinders with a height of about 1 to 1.5 times the diameter: a compact shape that holds heat well and is easy to mould and cut off. Spherical blind risers are used where moulding allows, because they freeze slowest for their volume.

GATE 2026 · ME · Q.30MCQ · 1 markCasting

Match the casting defects dross, scab and scar to their descriptions.

In relation to metal casting defects, match the following
  • P. Dross · Q. Scab · R. Scar
  • I. Shallow blow found on a flat casting surface · II. Lighter impurities appearing on the top surface of a casting · III. A rough, thin layer of metal, protruding above the casting surface, on top of a thin layer of sand
  1. (A)P−II, Q−III, R−I
  2. (B)P−II, Q−I, R−III
  3. (C)P−III, Q−I, R−II
  4. (D)P−III, Q−II, R−I

Answer: (A) Official key: A

  1. Dross: light oxides and impurities that float up and get trapped near the top surface (II).
  2. Scab: a patch of the mould face lifts away, metal runs behind it, and a rough thin layer of metal ends up over a layer of sand (III).
  3. Scar: a shallow blow on a flat surface (I).

Option (A).

Where this shows up in industry

Foundries log defects by these names on scrap reports. Scabs point to mould sand that expands too much or is rammed too hard, and dross points to turbulent pouring or poor skimming, so naming the defect tells the team which process to fix.

GATE 2022 · ME Set-1 · Q.56NAT · 2 marksMetal forming

Aluminium sheet, 4 mm thick, rolled at the maximum draft with μ = 0.1. What is the roll separation force?

A 4 mm thick aluminum sheet of width is rolled in a two-roll mill of roll diameter 200 mm each. The workpiece is lubricated with a mineral oil, which gives a coefficient of friction, . The flow stress () of the material in MPa is , where is the true strain. Assuming rolling to be a plane strain deformation process, the roll separation force () for maximum permissible draft (thickness reduction) is _________ kN (round off to the nearest integer).
Use: where is average flow stress, is roll-workpiece contact length, and is the average sheet thickness.

Answer: 350 kN Official key: 340 to 360

  1. Maximum draft: , so the sheet goes from 4 to 3 mm.
  2. Contact length ; .
  3. True strain . Average flow stress .
  4. .

Using the final flow stress () instead of the average gives 429 kN, which is outside the key range.

Where this shows up in industry

Roll force sets the mill's motor, bearing and housing size, and it bends the rolls. Mill engineers grind rolls with a slight camber, or bend them hydraulically, so the sheet comes out flat across its width despite that force.

GATE 2022 · ME Set-2 · Q.58NAT · 2 marksMetal forming

A 100 mm billet is extruded into an L-section bar. What is the maximum force at the start?

A cylindrical billet of 100 mm diameter and 100 mm length is extruded by a direct extrusion process to produce a bar of L-section. The cross sectional dimensions of this L-section bar are shown in the figure. The total extrusion pressure () in MPa for the above process is related to extrusion ratio () aswhere is the mean flow strength of the billet material in MPa, is the portion of the billet length remaining to be extruded in mm, is the initial diameter of the billet in mm, and is the die shape factor.
If the mean flow strength of the billet material is 50 MPa and the die shape factor is 1.05, then the maximum force required at the start of extrusion is ________ kN (round off to one decimal place).
L-section bar: a 10 mm wide vertical leg 60 mm tall and a 10 mm thick horizontal leg 50 mm long, sharing the corner10 mm60 mm50 mm10 mm

Answer: 2429.3 kN Official key: 2426.0 to 2432.0

  1. L-section area: (the corner square is counted once). Billet area: .
  2. Extrusion ratio , .
  3. At the start the whole billet remains: , . .
  4. The ram pushes on the billet area: .

The force is highest at the start because friction between the billet and container acts on the full length (the term). Multiplying by the product area instead gives only 309.3 kN.

Where this shows up in industry

Direct-extrusion presses are rated by this peak breakthrough force, from small presses for aluminium window profiles to presses of several thousand tonnes for large EV battery-tray profiles. Indirect extrusion removes the billet-container friction term, which is why it needs less force for the same profile.

GATE 2024 · ME · Q.29MCQ · 1 markMetal forming

Which metal forming process is earing associated with?

The “Earing” phenomenon in metal forming is associated with
  1. (A)deep drawing
  2. (B)rolling
  3. (C)extrusion
  4. (D)forging

Answer: (A) Official key: A

  1. Rolled sheet has different properties in different directions in its plane (planar anisotropy).
  2. When a round blank is deep drawn into a cup, the flange draws in faster in some directions than others, and the cup rim ends up wavy, with peaks called ears: option (A).

Ears form at 0°/90° or at 45° to the rolling direction, depending on the sign of the planar anisotropy .

Where this shows up in industry

Beverage-can makers trim the ears off every drawn cup, so earing is scrap. Aluminium can-body sheet is processed to keep earing to a few percent of cup height, and suppliers test it with a standard cup draw before shipping.

GATE 2024 · ME · Q.62NAT · 2 marksMetal forming

A 20 mm disc is blanked from 2 mm sheet with allowance 0.04. What punch size is needed?

A blanking operation is performed on C20 steel sheet to obtain a circular disc having a diameter of 20 mm and a thickness of 2 mm. An allowance of 0.04 is provided. The punch size used for the operation is ___________ mm (rounded off to 2 decimal places).

Answer: 19.84 mm Official key: 19.84 to 19.92

  1. In blanking the disc is the product, so the die is made to the blank size: 20 mm.
  2. Clearance per side .
  3. .

The key range runs to 19.92 mm, which accepts reading 0.08 mm as the total clearance. In piercing it is the other way round: the punch is the hole size and the die is larger.

Where this shows up in industry

Press-tool designers pick clearance as a percentage of sheet thickness, commonly about 5-10% per side for mild steel. Too little wears the punch and needs more force; too much leaves a big burr and rollover on the blank edge.

GATE 2025 · ME · Q.39MCQ · 2 marksMetal forming

Ideal wire drawing of a perfectly plastic metal: what is the maximum reduction per pass?

Wire drawing operation is performed on a perfectly plastic metal without any strain hardening. Assuming no friction and no redundant work, the maximum possible percentage reduction in area in a single pass is closest to
  1. (A)51.2
  2. (B)63.2
  3. (C)75.0
  4. (D)93.2

Answer: (B) Official key: B

  1. With no friction or redundant work, the drawing stress is .
  2. The drawn wire must not yield, so : , .
  3. Maximum reduction : option (B).
Where this shows up in industry

Real wire lines take far smaller steps, often about 15-30% per die, because friction and redundant work use up much of the margin. Copper wire for cables passes through a dozen or more dies in one machine to reach its final size.

GATE 2025 · ME · Q.41MCQ · 2 marksMetal forming

Can a 30 mm plate be rolled to 27 mm in one pass with 500 mm rolls and μ = 0.12?

A plate of 30 mm thickness is fed through a rolling mill with two powered rolls. Each roll has a diameter of 500 mm. The plate thickness is to be reduced to 27 mm in a single pass. Assume no change in width. The process feasibility and the maximum draft (in mm) can be represented, respectively, as
Use the coefficient of friction as 0.12
  1. (A)feasible and 3.6
  2. (B)NOT feasible and 2.6
  3. (C)feasible and 3.0
  4. (D)NOT feasible and 6.0

Answer: (A) Official key: A

  1. The rolls can only drag the plate in if the draft is no more than .
  2. The required draft is , below 3.6 mm, so the pass is feasible: option (A).

Check with the bite angle: a 3 mm draft needs , less than . Option (C) quotes the required draft, not the maximum.

Where this shows up in industry

Hot strip mills plan the reduction for every stand from this bite limit and the motor power. Roughing stands often have knurled or grooved rolls to raise friction, so they can take bigger bites in the first passes.

GATE 2026 · ME · Q.59NAT · 2 marksMetal forming

30% stretching in length gives 15% thinning. What is the sheet's normal anisotropy?

In a deep drawing operation of a rectangular sheet metal, 30% stretching in length results in 15% reduction in thickness. Assuming volume constancy, the normal anisotropy of the sheet metal is ________ (rounded off to 2 decimal places).

Answer: 0.61 Official key: 0.59 to 0.63

  1. True strains: , .
  2. Volume constancy: .
  3. Normal anisotropy .

With engineering strains instead (width ratio ), you get -0.63, outside the key range. True strains add up to zero; engineering strains do not.

Where this shows up in industry

R below 1 means the sheet thins easily, which is typical of aluminium alloys and limits how deep they can be drawn. Deep-drawing steels for car panels are made with R around 1.6-2 or more, which resists thinning and allows deeper draws.

GATE 2022 · ME Set-1 · Q.57NAT · 2 marksWelding and joining

GTAW at 20 V, 150 A, 5 mm/s with 60% filler in the bead. What is the wire feed rate?

Two mild steel plates of similar thickness, in butt-joint configuration, are welded by gas tungsten arc welding process using the following welding parameters.
  • Welding voltage: 20 V
  • Welding current: 150 A
  • Welding speed: 5 mm/s
A filler wire of the same mild steel material having 3 mm diameter is used in this welding process. The filler wire feed rate is selected such that the final weld bead is composed of 60% volume of filler and 40% volume of plate material. The heat required to melt the mild steel material is 10 J/mm3. The heat transfer factor is 0.7 and melting factor is 0.6. The feed rate of the filler wire is __________ mm/s (round off to one decimal place).

Answer: 10.7 mm/s Official key: 10.5 to 10.9

  1. Heat reaching the work: . Of that, the melting factor 0.6 goes into melting: 1,260 W.
  2. Metal melted: . The filler is 60% of it: 75.6 mm3/s.
  3. Wire area: . Feed rate .

The welding speed is not needed for the feed rate (it would give the bead area, 25.2 mm2). Feeding the whole bead from the wire gives 17.8 mm/s.

Where this shows up in industry

Welding procedure specifications (WPS) fix the current, voltage, travel speed and wire feed together, because the filler-to-base-metal ratio (dilution) controls the weld metal's chemistry. Dilution matters most when joining stainless to carbon steel or cladding with a corrosion-resistant layer.

GATE 2022 · ME Set-2 · Q.57NAT · 2 marksWelding and joining

A 100 V open-circuit, 1000 A short-circuit source and V = 10 + 5l. What is the maximum arc power?

In a direct current arc welding process, the power source has an open circuit voltage of 100 V and short circuit current of 1000 A. Assume a linear relationship between voltage and current. The arc voltage () varies with the arc length () as , where is in volts and is in mm. The maximum available arc power during the process is _________ kVA (in integer).

Answer: 25 kVA Official key: 25 to 25

  1. Power source line: , so .
  2. Arc power . at , where .
  3. .

The arc characteristic only tells you the arc length that gives 50 V: . A brute-force search over arc lengths gives the same maximum.

Where this shows up in industry

Manual stick and TIG sets use this drooping (constant-current) characteristic so the current barely changes when the welder's hand moves and the arc length changes. MIG/MAG sets use a flat (constant-voltage) characteristic instead, so the arc corrects its own length as the wire feeds.

GATE 2024 · ME · Q.32MCQ · 1 markWelding and joining

What electrode material is used to weld low alloy steels by GMAW?

The most suitable electrode material used for joining low alloy steels using Gas Metal Arc Welding (GMAW) process is
  1. (A)copper
  2. (B)cadmium
  3. (C)low alloy steel
  4. (D)tungsten

Answer: (C) Official key: C

  1. In GMAW (MIG/MAG) the electrode is a consumable wire that melts and becomes the weld metal.
  2. So it must match the base metal's chemistry and strength: a low alloy steel wire, option (C).

Tungsten is the non-consumable electrode of GTAW (TIG). Copper is used for the contact tip and as a thin coating on steel wire, not as the filler.

Where this shows up in industry

Filler wires are chosen from standard classifications. For low alloy steels, an AWS ER80S-series wire such as ER80S-D2 (molybdenum-bearing) is a common choice, matched to the steel's strength and to any post-weld heat treatment.

GATE 2025 · ME · Q.21MCQ · 1 markWelding and joining

Which welding process is used to make tailor-welded blanks for cars?

The welding process commonly used for fabricating tailor-welded blanks of dissimilar thickness for automotive applications is
  1. (A)gas welding
  2. (B)laser welding
  3. (C)arc welding
  4. (D)friction welding

Answer: (B) Official key: B

  1. A tailor-welded blank joins sheets of different thickness or grade edge to edge before stamping, so the weld must be narrow, flat and strong enough to survive the press.
  2. Laser welding gives a narrow seam with a small heat-affected zone and little distortion, at high speed: option (B).
Where this shows up in industry

Door inner panels and B-pillars are classic tailor-welded blanks: thick or high-strength steel only where the hinges or crash loads need it, thinner sheet elsewhere. That cuts weight and the number of reinforcement parts in the body-in-white.

GATE 2025 · ME · Q.33NAT · 1 markWelding and joining

85% of a 2500 W beam falls within 5 mm and 65% within 3 mm. What is the power density in the ring?

During a welding operation, thermal power of 2500 W is incident normally on a metallic surface. As shown in the figure below (figure is NOT to scale), the heated area is circular. Out of the incident power, 85% of the power is absorbed within a circle of radius 5 mm while 65% is absorbed within an inner concentric circle of radius 3 mm. The power density in the shaded area is _________ W mm-2 (rounded off to 2 decimal places).
Circular heated area: an inner circle of radius 3 mm inside an outer circle of radius 5 mm; the ring between them is shaded3 mm5 mm

Answer: 9.95 W/mm² Official key: 9.92 to 9.98

  1. Power in the ring: .
  2. Ring area: .
  3. Power density .

Spreading the 85% over the whole 5 mm circle gives 27.1 W/mm2, the average, not the ring's value.

Where this shows up in industry

Power density decides what a heat source can do: an arc delivers roughly 5-500 W/mm2, while laser and electron beams go past 10,000 W/mm2 and can drill a keyhole through the joint. Welding simulation models the source as a Gaussian or double-ellipsoid distribution fitted to rings like these.

From GATE prep to a design and manufacturing career

Talk to a counsellor.

Talk to a career counsellor

Free 20-minute call. We'll map the right course to where you want to work.

By submitting you agree to our Terms and Privacy Policy.

Talk to a career counsellor

Talk to a career counsellor

Free 20-minute call. We'll map the right course to where you want to work.

By submitting you agree to our Terms and Privacy Policy.