Johnson-Cook calculator: flow stress, parameter fit, failure strain and impact heating
The Johnson-Cook model gives a metal's flow stress as σ = (A + Bεpⁿ)(1 + C ln ε̇*)(1 − T*ᵐ): strain hardening, times strain rate hardening, times thermal softening. For 1006 steel (Johnson and Cook, 1983) at a plastic strain of 0.2 and 1,000 /s that is 580.7 MPa at 293 K (20 °C) and 463.2 MPa at 600 K. Pick one of the paper's 12 metals or type your own constants, rate, temperature and unit system. Free, runs in your browser.
Other tabs fit A, B and n to your stress-strain data, convert to a Radioss LAW36 table or LAW2 Iflag = 1 input, give the Johnson-Cook failure strain D1-D5 against triaxiality, and hand-check a bullet hitting a bucket. The last tab checks the Radioss material laws challenge of Skill-Lync's crashworthiness course and the Ansys bullet challenge, built after reading all 390 public reports of them. For the ballistic limit, residual speed and Ansys set-up of the bullet challenge, use the bullet penetration calculator; for Johnson-Cook in metal cutting, the Merchant circle calculator.
Johnson and Cook 1983 · Altair Radioss reference and examples · Ansys Explicit Dynamics guide · Zhou, Wang and Wen 2019 · checked against a separate solution (1,860 checks at build) · Updated 23 Nov 2026
Presets fill A to Tm in the unit system you pick; typing a constant switches to Custom. Johnson and Cook fitted at ε̇0 = 1 /s: in a millisecond system that is 0.001 /ms. Tr is room temperature (Radioss's default is 300 K). The Radioss plate is Altair's RD-E 2601 example: a 290, b 562.3, n 0.63, σmax 425 MPa, no rate effect.
The default data are the challenge's LAW36 curve, as 10 reports type it. Engineering data are converted to true stress and plastic strain first (needs E). Iflag 1 defaults are Altair's own LAW2 example, which it also gives as a = 270, b = 450, n = 0.6.
σ* is mean stress over von Mises: −1/3 uniaxial compression, 0 shear, 1/3 uniaxial tension, 0.577 plane-strain tension, 2/3 equibiaxial tension. Zhou, Wang and Wen's table gives D1 to D3 only, so D4 and D5 are 0 in those presets (no rate or temperature effect on εf).
No report types the bullet's size, so 10 mm by 30 mm is a plain example: type yours. Tantalum 16,678 kg/m³. The strain rate is your guess; speed over element size is a fair start (139 m/s over 10 mm = 13,900 /s). Linear defaults: Copper Alloy NL's yield 280 MPa and tangent modulus 1,150 MPa as the Ansys bending reports type them (see the springback calculator), as a plastic slope E·Et/(E − Et); density 8,300 and specific heat 385 as one bullet report types them.
Radioss defaults are what the reports read for case 1 (0.147 and 424.7 MPa). Bullet defaults are one report's 1006 steel bucket (plastic strain 1.402, 283.3 MPa, 591 °C). The heating estimate starts at 20 °C with 90% of the plastic work.
| Quantity | Equation | Value | From |
|---|---|---|---|
| Strain hardening f₁ | 504.1 MPa | A 350, B 275, n 0.36 | |
| Rate ratio | 1000 | ε̇ 1000 /s over ε̇0 1 /s | |
| Rate factor f₂ | 1.152 | C 0.022 | |
| Homologous temperature | 0 | Tm 1811 K | |
| Thermal factor f₃ | 1 | m 1 | |
| Flow stress | 580.7 MPa | no σmax |
- No σmax or EPS_p_max typed: the curve rises for ever.
| εp | σ data | σ fit | diff |
|---|---|---|---|
| 0 | 300 | 300 | 0 (not fitted) |
| 4.844e−4 | 360.1 | 361.1 | -0.9605 |
| 0.001119 | 390.6 | 388.6 | 1.991 |
| 0.00321 | 442.8 | 441.4 | 1.426 |
| 0.004781 | 466 | 468.7 | -2.747 |
- A = 300 MPa (the first point). B and n are a least-squares line through ln(σ − A) against ln εp over 4 points: R² = 0.9982 on the logs, 0.9979 on the stresses.
- The data stop at εp = 0.004781. A crash or impact run goes far past that, so the stress there comes from extrapolation: at 0.1 the last segment extended gives 1870 MPa, the Johnson-Cook fit 950.3 MPa; at 0.151 the last segment extended gives 2622 MPa, the Johnson-Cook fit 1081 MPa; at 0.16 the last segment extended gives 2754 MPa, the Johnson-Cook fit 1101 MPa.
LAW36 function (plastic strain, stress MPa) from the fit:
0 300 0.01 534.09 0.02 618.38 0.05 778.11 0.1 950.28 0.151 1080.75 0.2 1184.45 0.3 1358.78 0.5 1628.15
| LAW2 Iflag 1 | Value |
|---|---|
| a (yield) | 270 MPa |
| b | 450 MPa |
| n | 0.6001 |
| True stress at UTS | 467.5 MPa |
| True strain at UTS | 0.2535 |
| Your fit necks at | UTS 1010 MPa, engineering strain 0.4204 |
| State | σ* | εf | Deleted at |
|---|---|---|---|
| uniaxial compression | -0.3333 | 0.2419 | 0.151 (EPS_p_max) |
| pure shear | 0 | 0.19 | 0.151 (EPS_p_max) |
| uniaxial tension | 0.3333 | 0.1585 | 0.151 (EPS_p_max) |
| plane-strain tension | 0.5774 | 0.1436 | 0.1436 (card) |
| equibiaxial tension | 0.6667 | 0.1394 | 0.1394 (card) |
- Uniaxial tension: εf = 0.1585, so EPS_p_max = 0.151 deletes the element first. Equibiaxial: εf = 0.1394, so the failure card deletes it first.
- At σ* = 0.3333 and εp = 0.1: εf = 0.1585, damage D = εp/εf = 0.6308 (constant triaxiality; in a run D adds up Δεp/εf step by step).
| Quantity | Value |
|---|---|
| Bullet volume | 2356 mm³ |
| Bullet mass | 39.3 g |
| Speed | 139 m/s |
| Kinetic energy | 379.6 J |
| Momentum | 5.462 kg·m/s |
| Free travel v·t | 1390 mm |
| Bucket model | 1006 steel |
| Plastic work | 869.9 MJ/m³ |
| Temperature rise | 219.5 K (no softening: 237.1 K) |
| Flow stress at start / end | 423.5 / 679.3 MPa |
| Melted | no |
- In 0.01 s the bullet travels 1390 mm if it keeps its speed. Ansys's maximum total deformation is usually the bullet's own travel, not the bucket's.
- Case 1: LAW2 with EPS_p_max 0.151 and /FAIL/JOHNSON (elements deleted).
- The plate is LAW2 with a = 290, b = 562.3, n = 0.63 and σmax = 425 MPa (Altair's RD-E 2601 values, which 10 reports quote as 425). The curve reaches 425 MPa at εp = 0.1039 and stays there.
- Your 424.7 MPa sits at the 425 MPa cap: the plate is past εp = 0.1039 where it hits.
- εp = 0.147 below 0.151 is what you should see: elements that reached 0.151 were deleted and their strain is no longer plotted. 3 reports ask why their maximum (0.147) is below 0.151; this is why.
- /FAIL/JOHNSON (D1 0.11, D2 0.08, D3 −1.5): εf = 0.1585 in uniaxial tension, above EPS_p_max = 0.151, so 0.151 deletes those elements first. Equibiaxial εf = 0.1394 is below 0.151: there the failure card acts first.
- 0.0028 g/mm³ = 2800 kg/m³: aluminium, right. In mm, ms, g the plate's density is about 0.0027 to 0.0028 g/mm³.
Examples: a report asking why its maximum is 0.147, a report typing the LAW2 constants, the bullet report with 22 °C iron and 591 °C steel.
What is the Johnson-Cook model?
Johnson and Cook wrote the von Mises flow stress as three brackets: strain hardening, strain rate hardening and thermal softening. Every quantity in it is one an impact code already tracks:
A is the yield stress and B and n the hardening. The first bracket is the stress at ε̇* = 1 and room temperature. In the paper ε̇0 = 1.0 /s. T* runs from 0 at room temperature to 1 at melting, where the stress is zero. Ansys: "the yield stress drops to zero at the melting temperature". The second and third brackets scale the whole curve. For 1006 steel at εp = 0.2, 1,000 /s lifts the stress by 15.2% and 600 K takes off 20.22%.
Radioss's LAW2 adds two limits. σmax caps the stress (with the rate factor if ICC = 1), and EPS_p_max deletes a shell once one integration point reaches it:
Below ε̇0 Radioss applies no rate effect at all: "If ε̇ ≤ ε̇0, no strain rate effect". In the original form the logarithm goes negative there. The first tab offers both. If T is below the reference, T* is negative; the Radioss reference does not say what happens, so the calculator uses T* = 0.
What are the Johnson-Cook parameters for steel, aluminium and copper?
Johnson and Cook's 1983 Table 1 gives the constants for 12 metals, from torsion tests over a wide range of rates and Hopkinson bar tests up to high temperatures. The last two columns are the calculator's flow stress at εp = 0.2 and 1,000 /s, at 293 K and at 600 K:
| Material | ρ (kg/m³) | c (J/kg·K) | Tm (K) | A (MPa) | B (MPa) | n | C | m | σ, 293 K | σ, 600 K |
|---|---|---|---|---|---|---|---|---|---|---|
| OFHC copper | 8,960 | 383 | 1,356 | 90 | 292 | 0.31 | 0.025 | 1.09 | 313.5 | 232.5 |
| Cartridge brass | 8,520 | 385 | 1,189 | 112 | 505 | 0.42 | 0.009 | 1.68 | 391.8 | 327 |
| Nickel 200 | 8,900 | 446 | 1,726 | 163 | 648 | 0.33 | 0.006 | 1.44 | 566.5 | 504.9 |
| Armco iron | 7,890 | 452 | 1,811 | 175 | 380 | 0.32 | 0.06 | 0.55 | 568.7 | 332.6 |
| Carpenter electrical iron | 7,890 | 452 | 1,811 | 290 | 339 | 0.4 | 0.055 | 0.55 | 645.9 | 377.7 |
| 1006 steel | 7,890 | 452 | 1,811 | 350 | 275 | 0.36 | 0.022 | 1 | 580.7 | 463.2 |
| 2024-T351 aluminium | 2,770 | 875 | 775 | 265 | 426 | 0.34 | 0.015 | 1 | 564.5 | 204.9 |
| 7039 aluminium | 2,770 | 875 | 877 | 337 | 343 | 0.41 | 0.01 | 1 | 549.8 | 260.8 |
| 4340 steel | 7,830 | 477 | 1,793 | 792 | 510 | 0.26 | 0.014 | 1.03 | 1237 | 995.3 |
| S-7 tool steel | 7,750 | 477 | 1,763 | 1539 | 477 | 0.18 | 0.012 | 1 | 2053 | 1624 |
| Tungsten alloy (.07Ni, .03Fe) | 17,000 | 134 | 1,723 | 1506 | 177 | 0.12 | 0.016 | 1 | 1834 | 1441 |
| DU-.75Ti | 18,600 | 117 | 1,473 | 1079 | 1120 | 0.25 | 0.007 | 1 | 1916 | 1418 |
Johnson and Cook could not explain 1006 steel's high-temperature data and took m = 1.00 for it; five of the metals came from torsion data only. A, B and n are averages of torsion and tension fits, "generally within about 10 percent" of either. The 2024-T351 aluminium melts at 775 K, so 600 K already takes off most of its strength.
What ε̇0, density and stress units do I type in Radioss?
Radioss has no unit system of its own: the numbers must agree. The material laws challenge runs in mm, ms and g, so stress comes out in MPa (N/mm²) but time is in milliseconds:
| System (stress, time; length, mass) | Stress | Rate | Aluminium density | ε̇0 = 1 /s is |
|---|---|---|---|---|
| MPa, s (mm, t) | MPa | 1/s | 2.700e−9 t/mm³ | 1 1/s |
| MPa, ms (mm, g) | MPa | 1/ms | 0.0027 g/mm³ | 0.001 1/ms |
| Pa, s (SI) | Pa | 1/s | 2700 kg/m³ | 1 1/s |
| GPa, ms (mm, kg) | GPa | 1/ms | 2.700e−6 kg/mm³ | 0.001 1/ms |
The slip to watch is ε̇0. Typed as 1 in a millisecond deck it means 1 /ms = 1,000 /s, and Radioss then ignores the rate effect below 1,000 /s. For cartridge brass at εp = 0.2 and 500 /s (0.5 /ms) that silently drops the rate factor 1.056 to 1. The challenge's plate has no rate term, so it does not matter there, but it will in your next model. Density is the other: 0.0027 g/mm³ is 2,700 kg/m³ (39 reports type 0.0027 and 58 type 0.0028).
How do I fit A, B and n to my stress-strain data?
Johnson-Cook wants true stress against plastic strain. Engineering data convert first (valid up to necking):
Take A as the yield (the first point of a plastic-strain table, or the stress at 0.2% plastic strain). Then B and n fall out of a straight line through the logs:
The challenge's LAW36 curve gives A = 300 MPa, B = 1806 MPa and n = 0.4437, with R² = 0.9982 on the logs. The fit is good where the data are, but the data stop at εp = 0.004781. The plate goes to 0.1 and beyond. Radioss: "Beyond the last point of the plastic strain versus stress input curves, the yield stress is extrapolated." Where it ends up depends on how you extend it:
| Plastic strain | Last segment extended (slope 14,744 MPa) | Johnson-Cook fit |
|---|---|---|
| 0.1 | 1870 MPa | 950.3 MPa |
| 0.151 | 2622 MPa | 1081 MPa |
| 0.16 | 2754 MPa | 1101 MPa |
The Radioss reference says the curve is extrapolated but not how; the calculator extends the last segment, which is an assumption. Either way the answer at εp = 0.1 is a guess two to four times the last point. Give the table points out to the strains your run reaches. The second tab writes a LAW36 table from a Johnson-Cook curve at the strains you list.
What does Iflag = 1 do in Radioss LAW2?
With Iflag = 1 you type the yield stress, the engineering UTS and the engineering strain at UTS, and Radioss prints a, b and n in the Starter output. The reference page does not give the formula. Necking starts at UTS, where the slope of the true curve equals the stress (Considère). With a = σy and the true values at UTS
This reproduces Altair's own pair of LAW2 examples for the same steel. Yield 270 MPa, UTS 362.8 MPa and 0.2885 give n = 0.6001 and b = 450 MPa. The classic example types a = 270, b = 450, n = 0.6, and back the other way that curve necks at UTS 362.8 MPa and engineering strain 0.2885. The elastic strain is left out, as the match shows Altair does. Radioss requires n ≤ 1: a large strain at UTS with a small UTS/yield ratio breaks that. The challenge plate (a 290, b 562.3, n 0.63) would neck at UTS 409.9 MPa, but its σmax of 425 MPa caps the true stress first, at εp = 0.1039.
What is the Johnson-Cook failure model (D1 to D5)?
The failure card gives the plastic strain at fracture as a function of stress triaxiality σ*, strain rate and temperature, and adds up damage step by step:
With σ* as mean stress over von Mises (Radioss and Ansys both write it so), D3 is negative: more tension, less ductility. The challenge's card is Altair's RD-E 2602 example, with no rate or temperature terms:
| Shell stress state | σ* | εf | With EPS_p_max = 0.151, deleted at |
|---|---|---|---|
| uniaxial compression | −1/3 | 0.2419 | 0.151 (EPS_p_max) |
| pure shear | 0 | 0.19 | 0.151 (EPS_p_max) |
| uniaxial tension | 1/3 | 0.1585 | 0.151 (EPS_p_max) |
| plane-strain tension | 1/√3 = 0.577 | 0.1436 | 0.1436 (failure card) |
| equibiaxial tension | 2/3 | 0.1394 | 0.1394 (failure card) |
Altair's example says it in one line: εf = 0.1585 at σ* = 1/3, and the element fails "once reach the smallest failure strain either defined with εpmax in LAW2 or D = 1 in /FAIL/JOHNSON". So in tension and shear EPS_p_max = 0.151 deletes first. Only in plane-strain and biaxial tension, where εf drops to 0.1436 and 0.1394, does the failure card act first.
Published sets read for this page (D4 and D5 are not in that table):
| Material (Zhou, Wang and Wen 2019, Table 1) | D1 | D2 | D3 | εf shear | εf uniaxial | εf biaxial |
|---|---|---|---|---|---|---|
| OFHC copper | 0.54 | 4.89 | -3.03 | 5.43 | 2.321 | 1.189 |
| 4340 steel | 0.05 | 3.44 | -2.12 | 3.49 | 1.747 | 0.8871 |
| 2024-T351 aluminium | -0.07 | 1.02 | -1.62 | 0.95 | 0.5244 | 0.2764 |
- Ifail_sh = 1 (default): "Shell is deleted or cracked when D ≥ 1 for one integration point or layer." = 2: only when all layers have failed; Altair's plate shows "less failure" with 2.
- Ixfem = 1: "the failure criteria will lead to element cracking instead of element or layer deletion", for QEPH (Ishell 24) and BT shells only.
- Dadv: with XFEM, a new crack starts in an element at D > 1; a crack already in a neighbour advances into it once D > Dadv (default 1).
LAW2, LAW36, LAW27 or LAW1: what changes in the Radioss challenge?
The challenge hits an aluminium plate with a rigid sphere and runs seven cases. What each law does with the same plate:
| Case | Law and change | What limits the stress | What removes elements |
|---|---|---|---|
| 1 | LAW2 + /FAIL/JOHNSON | σmax 425 MPa, reached at εp 0.1039 | EPS_p_max 0.151 (tension, shear); D = 1 in biaxial zones |
| 2 | same, Ifail_sh 1, Dadv 1, Ixfem 1 | σmax 425 MPa | cracks (XFEM) instead of deletion |
| 3 | /FAIL/JOHNSON deleted | σmax 425 MPa | EPS_p_max 0.151 only |
| 4 | EPS_p_max deleted too | σmax 425 MPa | nothing (default 10²⁰) |
| 5 | LAW1, elastic (ρ 0.0028, E 71,000, ν 0.33) | nothing: no yield | nothing |
| 6 | LAW27, brittle damage | Johnson-Cook, then damage from principal total strain εt | principal strain past εf, tension only |
| 7 | LAW36, the given curve | the table, extrapolated past εp 0.004781 | Eps_t 0.1 / Eps_m 0.11 soften first; EPS_p_max 0.16 |
Why case 3 looks almost like case 1: 0.151 deleted the tension and shear elements before the failure card could, so removing the card changes only the biaxial zones. One report puts it plainly: "Thus even after deleting the /FAIL/JOHNSON card, we can see almost same results". And σmax is a cap, not a failure stress. With EPS_p_max deleted the plate holds 425 MPa and keeps straining; 4 reports read 425 as the stress at which elements fail.
LAW27 and LAW36's εt, εm and εf are total principal strains; LAW2's EPS_p_max is plastic. Altair matches them with total = σy/E + εp: 290/71,000 + 0.1559 = 0.16.
Bullet penetrating a bucket: what should the numbers be?
The Ansys challenge fires a tantalum bullet at 139 m/s into a fixed bucket for 0.01 s. A 10 mm by 30 mm tantalum cylinder (an example; the reports give no size) weighs 39.3 g:
- Energy. 379.6 J at 139 m/s. Typed as 13,900 mm/s the speed is 13.9 m/s and the energy 3.796 J, one hundredth. 4 reports type 13,900 mm/s; 70 type 139,000 mm/s.
- Total deformation. In 0.01 s the bullet flies 1390 mm. 31 reports give a maximum deformation near 1,390 mm: that is the bullet, not the bucket. One report says so: the maximum is "the same as the distance that is traversed by the bullet in 0.01s".
- Plastic strain. Every one of the 15 maximum plastic strains typed in 5 reports lies between 1.242 and 1.49. Ansys erodes an element when its geometric strain passes 1.5 by default ("The default value of 1.5 can be used in most cases"), so the contour shows the elements that survived, not the ones at the hole.
The heat comes from plastic work. A Taylor-Quinney fraction β of it, "a typical assumption is that β = 0.9", warms the metal. With Johnson-Cook the warming softens the metal as it goes, so the integration is coupled:
At a plastic strain of 1.35 and 13,900 /s, starting from 20 °C:
| Bucket material | Temperature | Rise | Rise with no softening | Flow stress at the end |
|---|---|---|---|---|
| OFHC copper (JC) | 158.8 °C | 138.9 K | 146.7 K | 453 MPa |
| Armco iron (JC) | 224.7 °C | 204.9 K | 263.5 K | 622.8 MPa |
| 1006 steel (JC) | 239.4 °C | 219.5 K | 237.1 K | 679.3 MPa |
| 2024-T351 aluminium (JC) | 270.4 °C | 250.6 K | 353.6 K | 404.4 MPa |
| 4340 steel (JC) | 414.1 °C | 394.2 K | 453.4 K | 1138 MPa |
| Al 1100-O (Steinberg-Guinan, as typed) | 107.5 °C | 87.6 K | 87.6 K | 218.8 MPa |
| Copper Alloy NL (bilinear, no thermal term) | 424.6 °C | 404.7 K | 404.7 K | 1849 MPa |
Ansys's Steinberg-Guinan form for Al 1100-O, as one report types it (Y0 40 MPa, β 400, n 0.27, Ymax 480 MPa), has its temperature term through dG/dT, which the report does not give, so the table leaves it out:
Many reports use the General Non-linear materials (Aluminium Alloy NL, Copper Alloy NL, Stainless Steel NL): bilinear lines with no thermal softening term like Johnson-Cook's 1 − T*ᵐ. Nothing in them stops the heating: 12 of the 15 reports that type a temperature give one above 1,538 °C, where iron melts, and the highest is 15,225.5 °C. Johnson-Cook cannot do that, because its strength is zero at Tm.
22 °C means no heating, not a cool bucket. One report lists maxima of 328.8 °C for Al 1100-O, 22 °C for iron and 591 °C for steel 1006, at plastic strains of 1.348, 1.37, 1.402. Ansys: "Temperature will be non-zero only if a specific heat capacity is defined." The iron needs a specific heat. By hand, 90% of the plastic work at those strains gives 107.3 °C, 227.8 °C and 248.3 °C. The reported 329 °C and 591 °C are two to three times hotter, so treat the hand number as a check of the order, not of the peak element.
What did 390 reports do?
Skill-Lync read every public report of the two challenges on 23 Nov 2026. As of that date n = 390: 239 are the Radioss material laws challenge and 151 the bullet challenge (one more matched the search but is a bird strike project, left out). The median report has 1,025 words of text and 25 images; 3 are mostly images. Every count below is from the report text, so values typed only in screenshots are not counted.
| In the report text | Reports | Examples |
|---|---|---|
| Radioss: FAILURE_JOHNSON starter file named | 148 | 1, 2 |
| Radioss: EPS_p_max 0.151 stated | 85 | 1, 2 |
| Radioss: Ixfem / XFEM (case 2) named | 206 | 1, 2 |
| Radioss: LAW27 named | 218 | 1, 2 |
| Radioss: LAW36 named / its curve typed | 217 / 10 | 1, 2 |
| Radioss: density 0.0028 / 0.0027 g/mm³ typed | 58 / 39 | 1, 2 |
| Radioss: a 290, b 562.3, n 0.63 typed | 5 | 1, 2 |
| Radioss: σmax 425 MPa stated as a stress | 10 | 1, 2 |
| Bullet: tantalum bullet | 100 | 1, 2 |
| Bullet: 139,000 mm/s / 139 m/s typed | 70 / 18 | 1, 2 |
| Bullet: 13,900 mm/s typed (ten times slow) | 4 | 1, 2 |
| Bullet: end time 0.01 s | 55 | 1, 2 |
| Bullet: maximum deformation near 1,390 mm | 31 | 1, 2 |
| Bullet: Aluminium Alloy NL / Copper Alloy NL / Stainless Steel NL | 92 / 72 / 69 | 1, 2 |
| Bullet: Al 1100-O / steel 1006 / tungsten (explicit library) | 30 / 8 / 5 | 1, 2 |
| Bullet: magnesium / titanium / structural steel | 53 / 33 / 22 | 1, 2 |
- The deleted elements are why the maximum is under 0.151. 3 reports ask it outright: "But here the maximum strain shown here is 1.426E-01 which is 0.147,Why ?". Radioss removes a shell the moment one integration point reaches EPS_p_max, so its strain is gone from the plot.
- σmax read as a failure stress. 4 reports do, for example "which means that the failure would now occur only according the the max stress value SIG_max0". LAW2 caps the stress at σmax; only EPS_p_max or the failure card delete.
- 4 bullet reports type 13,900 mm/s. That is ten times slower than 139 m/s and a hundredth of the energy.
What this calculator does not cover
- Pressure and shock: the equation of state (Ansys's Shock EOS, Radioss /EOS) and the pressure terms of Steinberg-Guinan.
- Penetration mechanics: whether the bullet perforates, the residual velocity and the hole size need the run, or a ballistic limit model.
- Heat conduction: the heating is adiabatic, as Radioss assumes for LAW2 ("Adiabatic conditions are assumed for thermal simulations"). A slow test has time to lose heat.
- Strain path: the damage sum is done at constant triaxiality; a real element changes σ* as it deforms.
Picking a material law, setting failure that deletes the right elements and reading why a peak is where it is are what crash and impact teams test in interviews. The Radioss material laws challenge is part of Skill-Lync's crashworthiness course; the bullet challenge is in the Ansys Workbench course.
Frequently asked questions
What is the Johnson-Cook model?
A flow stress law for metals at large strains, high strain rates and high temperatures: σ = (A + Bεpⁿ)(1 + C ln ε̇*)(1 − T*ᵐ). Johnson and Cook published it in 1983 with constants for 12 metals. Crash and impact codes (Radioss LAW2, Ansys Explicit, LS-DYNA) use it because it needs only plastic strain, strain rate and temperature.
What are A, B, n, C and m in Johnson-Cook?
A is the yield stress, B and n the strain hardening, C the strain rate sensitivity at the reference rate ε̇0 (1 /s in the paper), and m the thermal softening exponent between room temperature and melting. For 1006 steel: A 350 MPa, B 275 MPa, n 0.36, C 0.022, m 1.00, melting 1,811 K.
What are the Johnson-Cook parameters for steel and aluminium?
From Johnson and Cook's 1983 table: 4340 steel A 792 MPa, B 510, n 0.26, C 0.014, m 1.03; 1006 steel 350, 275, 0.36, 0.022, 1.00; 2024-T351 aluminium 265, 426, 0.34, 0.015, 1.00; 7039 aluminium 337, 343, 0.41, 0.010, 1.00. The calculator holds all 12 metals with density and specific heat.
What is the Johnson-Cook failure model (D1 to D5)?
It gives the plastic strain at fracture: εf = [D1 + D2 exp(D3σ*)][1 + D4 ln ε̇*][1 + D5T*], with σ* the mean stress over von Mises. Damage D adds Δεp/εf each step and the element fails at D = 1. In the Radioss challenge D1 0.11, D2 0.08, D3 −1.5 give εf 0.1585 in uniaxial tension.
What is the difference between LAW2 and LAW36 in Radioss?
LAW2 (PLAS_JOHNS) is the Johnson-Cook equation: you type a, b, n, c and optional σmax and EPS_p_max. LAW36 (PLAS_TAB) takes the hardening as a table of yield stress against plastic strain, one curve per strain rate. Radioss extrapolates beyond the table's last point, so give points out to the strains your run reaches.
Why does my bullet simulation show no temperature rise?
Ansys computes temperature only when the material has a specific heat: "Temperature will be non-zero only if a specific heat capacity is defined." One report reads 22 °C for an iron bucket at a plastic strain of 1.37. With a specific heat, 90% of that plastic work would heat it by about 208 K.
Related on Skill-Lync
- True stress-strain calculator: engineering to true stress and plastic strain, the input the fit needs
- Yield strength calculator: the 0.2% offset yield that becomes A
- Explicit time step calculator: the Courant step and mass scaling of the same runs
- Shell element formulation calculator: Assignment 3 of the same course, hourglass modes, Ishell 24 and the energy error check
- Bullet penetration calculator: ballistic limit, residual speed and the Ansys set-up of the bullet challenge
- Merchant circle calculator: Johnson-Cook in the Ansys machining challenge
- Crash box calculator and drop test calculator: other explicit impact hand checks
- Hyperelastic curve fit calculator: the same kind of fit for rubber
- HyperMesh courses compared
- All free engineering tools
Sources
- G.R. Johnson and W.H. Cook, A constitutive model and data for metals subjected to large strains, high strain rates and high temperatures, 7th International Symposium on Ballistics, The Hague, 1983: the model, ε̇0 = 1 /s, Table 1 (12 metals with density, specific heat and melting point).
- Altair Radioss Reference Guide: /MAT/LAW2 (PLAS_JOHNS), /MAT/LAW36 (PLAS_TAB), /MAT/LAW27 (PLAS_BRIT), /FAIL/JOHNSON. Example Guide RD-E 2601 Failure Strain and RD-E 2602 Ductile Failure Model (the challenge's plate, D1-D3 and EPS_p_max).
- Ansys Explicit Dynamics Analysis Guide 2025 R2: Johnson-Cook Strength, Steinberg-Guinan Strength, Johnson-Cook Failure, Erosion Controls.
- L. Zhou, Z. Wang and H. Wen, On the Accuracy of the Johnson-Cook Constitutive Model for Metals, Chinese Journal of High Pressure Physics 33(4), 2019, Table 1 (D1-D3, after Johnson and Cook 1985). S.A. Silling and M. Fermen-Coker, Sandia report SAND2012-5091 (σ* and ef = D1 + D2 e^(D3/3)).
- Taylor-Quinney β = 0.9: arXiv 2305.18835. Wikipedia: Stress–strain curve (true stress and strain), Necking (engineering) (Considère), tantalum density 16.678 g/cm³.
- Skill-Lync, all 390 public reports of the two challenges, read 23 Nov 2026. scripts/verify/johnson_cook.py recomputes every case another way: the fit by the normal equations, the UTS by Newton's method, the heating by closed forms or a separate Heun integration, and Altair's and Johnson and Cook's numbers as hand cases. 115 cases; the page checks itself against it at build time (1,860 checks).