0.2% offset yield strength calculator

Paste your tensile test data, as stress and strain or as load and extension straight from the machine, and get the 0.2% offset yield strength (proof stress Rp0.2), Young's modulus, ultimate strength and elongation, with the offset line drawn on your curve. Any offset, toe correction included. Free, no sign-up, your data never leaves the browser.

ASTM E8/E8M offset method · ISO 6892-1 Rp, Rt · least-squares modulus · verified on 200 test curves · Updated 16 Nov 2026

Yield strength Rp0.2349.9 MPaat strain 0.375%
Young's modulus E199.3 GPafit on 7 points, R² 0.99999
01002003004005000.00.20.40.60.81.0Strain (%)Stress (MPa)Rp0.2 = 349.9 MPa— 0.2% offset line- - elastic fit (E)
Maximum stress (UTS if the test ran past it)480.5 MPa

    What is 0.2% offset yield strength?

    The 0.2% offset yield strength is the stress at which a metal has taken 0.2% permanent (plastic) strain. It is used for metals that yield gradually, such as aluminium, stainless steel and copper, where no clear yield point shows on the curve. ISO 6892-1 calls it Rp0.2, the 0.2% proof strength; datasheets list it as "yield strength".

    Why 0.2%? Up to a good fraction of the yield stress these metals are almost perfectly elastic; then plastic strain starts and grows quickly. No single stress marks "the" start, so the standards agree on a small, measurable permanent strain: 0.002 mm/mm, 0.1 mm over a 50 mm gauge length. Design codes, FEA material cards and supplier certificates then all quote the same number.

    How do you calculate 0.2% offset yield strength?

    Fit a straight line to the elastic part of the stress-strain curve, shift it 0.002 strain to the right, and read the stress where it crosses the curve. That crossing is Rp0.2. With a table of readings instead of a plot, there are four steps:

    1. Young's modulus. Least-squares fit of σ = Eε + c to the points in the straight part (this calculator uses 10% to 40% of the maximum stress by default; you can change the band). The intercept gives the toe correction ε0, the strain lost to slack and seating at the start of the test.
    2. Offset line. The line parallel to the elastic slope, starting at 0.2% strain past the corrected origin.
    3. Crossing. For each reading, gi = curve stress minus offset-line stress. It is positive while the curve is above the line and turns negative once the curve falls below it.
    4. Interpolate between the last positive and first negative reading.

    Interpolating on g, not just picking the nearest reading, matters when readings are sparse near yield: in worked example 2 the readings are 0.02 mm apart and the answer still lands within 0.1 MPa of the exact value.

    Worked example 1: a curve whose answer we know

    To test any method you need a curve with a known answer. The Ramberg-Osgood equation gives one: its plastic strain is exactly 0.002 when σ = S, so its 0.2% offset yield is S by construction. We sampled it with E = 200.0 GPa, S = 350 MPa and n = 10 (a steel-like curve) at 45 strain readings, rounded to 0.1 MPa. It is the steel sample in the calculator.

    The modulus fit uses the 7 readings between 48 and 192 MPa and gives E = 199.3 GPa (R² = 0.99999), slightly under the true 200.0 GPa because a little plastic strain already creeps in at 40% of the maximum. The offset line then crosses the curve at Rp0.2 = 349.86 MPa, 0.04% from the exact 350 MPa.

    0100200300400500012345Strain (%)Stress (MPa)Rp0.2 = 349.9 MPa— 0.2% offset line- - elastic fit (E)
    Full curve (to 5.0% strain): the elastic fit (dashed) and the 0.2% offset line (orange) are steep next to the plastic part.
    01002003004005000.00.20.40.60.81.0Strain (%)Stress (MPa)Rp0.2 = 349.9 MPa— 0.2% offset line- - elastic fit (E)
    Zoom on yield: the offset line meets the measured curve at 349.9 MPa. Dots are the readings.

    Worked example 2: from load-extension readings to Rp0.2

    Most lab reports start from a UTM printout of load and extension. Here is one for an aluminium alloy: round specimen, d0 = 12.5 mm, extensometer gauge length L0 = 50 mm, extension to 0.001 mm, load to 0.01 kN. (Readings generated from a Ramberg-Osgood curve with E = 69.0 GPa and S = 276 MPa, so the answer can be checked; it is the aluminium sample in the calculator.)

    Extension (mm)Load (kN)StrainStress (MPa)
    0.023.390.000427.6
    0.046.770.000855.2
    0.0610.160.001282.8
    0.0813.550.0016110.4
    0.1016.940.0020138.0
    0.1220.320.0024165.6
    0.1423.710.0028193.2
    0.1627.040.0032220.3
    0.1829.800.0036242.8
    0.2031.370.0040255.6
    0.2232.260.0044262.9
    0.2432.840.0048267.6
    0.2533.060.0050269.4
    0.2733.440.0054272.5
    0.2933.740.0058274.9
    0.3133.990.0062277.0
    0.3334.210.0066278.8
    0.3634.480.0072281.0
    0.4034.780.0080283.4
    0.5035.350.0100288.1

    Convert to stress and strain with the original area and gauge length (engineering values):

    Modulus. The maximum stress in the table is 288.1 MPa, so the fit band is 29 to 115 MPa: the 3 readings from 0.04 to 0.08 mm (shaded blue). Least squares gives E = 69,061 MPa = 69.1 GPa with R² = 1.000000 (in Excel: =SLOPE over those rows).

    Find the crossing. g changes sign between the readings shaded green, at 0.29 and 0.31 mm:

    So Rp0.2 = 275.9 MPa (exact 276 MPa), at a force of 33.86 kN. The 0.5% extension-under-load value on the same data is Rt0.5 = 269.4 MPa, lower than Rp0.2: for aluminium the elastic strain at yield (0.40%) is large, so 0.5% total strain comes before 0.2% plastic strain. For steel it is the other way round.

    0501001502002503000.00.20.40.60.81.0Strain (%)Stress (MPa)Rp0.2 = 275.9 MPa— 0.2% offset line- - elastic fit (E)
    Example 2 near yield: readings (dots), elastic fit (dashed) and offset line (orange) meeting the curve at 275.9 MPa.

    How to calculate 0.2% offset yield strength in Excel

    Copy the strain and stress columns of the example 2 table into columns A and B of a sheet, starting in row 2 (so rows 2 to 21). The whole method then takes four formulas:

    1. E in E1: =SLOPE(B3:B5,A3:A5) over the elastic rows. Stress is known_y's, strain is known_x's. Swapping them gives 1/E, a common mistake.
    2. Toe correction in E2: =-INTERCEPT(B3:B5,A3:A5)/E1 (near zero for clean data).
    3. g in C2, filled down: =B2-$E$1*(A2-$E$2-0.002).
    4. Interpolate between the last positive and the first negative g, here rows 16 and 17: =B16+C16/(C16-C17)*(B17-B16) gives 275.9 MPa.

    Plotting columns A and B with the line E1 × (A − E2 − 0.002) on the same chart is the graphical check; the calculator on this page does all of it and draws the plot. Paste the same two columns into it to check your sheet.

    Why 0.2%, and what do other offsets give?

    A bigger offset gives a higher value on any work-hardening curve, so the offset must always be stated. On worked example 1's curve:

    Offset (plastic strain)Symbol (ISO 6892-1)From the dataExact (Ramberg-Osgood)
    0.05%Rp0.05304.9 MPa304.7 MPa
    0.1%Rp0.1326.6 MPa326.6 MPa
    0.2%Rp0.2349.9 MPa350.0 MPa
    0.5%Rp0.5383.6 MPa383.6 MPa

    ISO 6892-1 writes the offset into the symbol (Rp0.1, Rp1), and European stainless-steel standards (EN 10088) list Rp1.0 next to Rp0.2 for austenitic grades. The extension-under-load method (Rt, stress at a total strain such as 0.5%) needs no modulus, which makes it quick on a test machine; ASTM E8/E8M describes it alongside the offset method. Use whichever your material specification names.

    What if the curve has a yield point, like mild steel?

    Then you don't need an offset. Low-carbon steel shows a stress drop and a plateau: ISO 6892-1 reports the upper yield strength ReH (the peak before the drop) and the lower yield strength ReL (the lowest stress on the plateau, ignoring the first dip). If you run the offset method on such a curve, the line usually meets it on the plateau, close to ReL. Read ReH and ReL from your data directly.

    Elongation, UTS and the yield-to-tensile ratio

    The calculator also reports the maximum stress (the ultimate tensile strength Rm, if your test went past the peak), the strain there (uniform elongation), and the permanent strain at the last reading, which is the elongation after fracture A if the test ran to fracture:

    The elastic part σlast/E recovers when the bar breaks, so it is subtracted. The ratio Rp0.2/Rm tells you how much the material work-hardens after yield: low ratios (around 0.4 to 0.7) mean lots of reserve strength, typical of annealed stainless and mild steels; ratios near 0.9 mean little, typical of high-strength aluminium alloys and quenched and tempered steels.

    What this calculator does not do

    • Validate your test. Specimen size, strain rate, extensometer class and alignment are set by ASTM E8/E8M or ISO 6892-1. A result is only as good as the strain measurement under it.
    • Crosshead strain. If E comes out far below the handbook value, the strain probably includes machine and grip stretch. The calculator warns you, but cannot correct it.
    • True stress-strain. All values are engineering (original area and length). FEA plasticity cards need true stress versus plastic strain; convert with σtrue = σ(1 + ε) up to the UTS.
    • Noisy data. The first crossing is used. Very noisy readings near yield can cross early; smooth the data or widen the fit band first.

    Use it to process lab data, check a spreadsheet, or learn the method. For certified results, follow the test standard your material specification calls up.

    Use material data in simulation

    Yield strength and the plastic curve go straight into FEA material cards. Skill-Lync's CAE courses teach how, on industry problems.

    Frequently asked questions

    How do you calculate 0.2% offset yield strength?

    Fit a straight line to the elastic part of the stress-strain curve to get Young's modulus E. Draw a parallel line shifted 0.002 strain to the right. The stress where that line crosses the curve is the 0.2% offset yield strength, Rp0.2. On a data table, find the first point where σ − E(ε − 0.002) turns negative and interpolate.

    What is the formula for 0.2% offset yield strength?

    There is no closed formula: it is read from the test curve. The offset line is σ = E(ε − 0.002), and Rp0.2 is the stress where the measured curve meets it. If the curve follows the Ramberg-Osgood equation ε = σ/E + 0.002(σ/S)^n, the 0.2% offset yield is exactly S.

    Why is 0.2% used for offset yield strength?

    Most metals have no sharp yield point, so a small, agreed permanent strain is used instead. 0.2% (0.002) is large enough to measure reliably with an extensometer and small enough to sit just past the end of elastic behaviour. It is the default in ASTM E8/E8M and ISO 6892-1, where it is written Rp0.2.

    What is the difference between yield strength and proof stress?

    Proof stress is the stress at a specified permanent (non-proportional) strain, such as 0.2%. For metals without a yield point, the 0.2% proof stress Rp0.2 is what datasheets report as the yield strength. Metals with a distinct yield point, like mild steel, report the upper and lower yield strengths ReH and ReL instead.

    How do you calculate 0.2% offset yield strength in Excel?

    Put strain in column A and stress in B. Get E with =SLOPE(B2:B9,A2:A9) over the elastic rows (stress is known_y, strain is known_x). In C2 enter =B2-$E$1*(A2-0.002) and fill down. Find the first row where C turns negative and interpolate between that row and the one above it.

    Why is my calculated Young's modulus much lower than the handbook value?

    Strain taken from the crosshead movement includes the stretch of the machine, grips and specimen shoulders, so E comes out far too low. An offset of 0.2% on that strain is then the wrong amount of plastic strain. Use extensometer strain for the modulus and the yield; crosshead data is fine for the overall curve shape.

    Is 0.2% offset yield strength the same as yield point?

    Not quite. A yield point is a visible event, a stress drop or plateau, seen in low-carbon steel. The 0.2% offset yield strength is a defined value for metals that yield gradually, like aluminium, stainless steel and copper. On a material with a plateau, the offset line usually meets the curve on the plateau, close to ReL.

    Related on Skill-Lync

    Sources

    • ASTM E8/E8M, Standard Test Methods for Tension Testing of Metallic Materials: yield strength by the offset method and the extension-under-load method.
    • ISO 6892-1:2019, Metallic materials: Tensile testing, Part 1: Method of test at room temperature: Rp (proof strength, plastic extension), Rt (total extension), ReH/ReL, Rm, A.
    • ASTM E111, Standard Test Method for Young's Modulus, Tangent Modulus, and Chord Modulus (least-squares fit of the linear region).
    • W. Ramberg and W. R. Osgood, Description of stress-strain curves by three parameters, NACA Technical Note 902, 1943.
    • Worked examples and all their numbers: Skill-Lync, recomputed by scripts/verify/offset_yield.py (pure Python; also 200 random Ramberg-Osgood curves with 0.1% load noise and 10 to 40 readings per yield strain, worst error 0.87%) and cross-checked against this page's calculator code at build time. Example data is generated, not from a real specimen.
    Free counselling

    Turn test data into simulation skills.

    Material models, plasticity and the FEA that uses them are what CAE interviews ask about. A Skill-Lync counsellor can map the course that fits the job you want.

    Talk to a CAE course counsellor

    Free. We call you back, usually the same day.

    By submitting you agree to our Terms and Privacy Policy.

    Talk to a career counsellor

    Talk to a career counsellor

    Free 20-minute call. We'll map the right course to where you want to work.

    By submitting you agree to our Terms and Privacy Policy.