Fatigue life calculator

Estimate how many load cycles a steel or aluminium part survives, the stress-life way. Enter the material, surface finish, size, notch and the load. You get the corrected endurance limit, the S-N curve, the fatigue safety factor and the life in cycles. Free, no sign-up, runs in your browser.

The mean stress is handled six ways side by side: Goodman, Gerber, Soderberg, ASME-elliptic, Morrow and Smith-Watson-Topper. The second tab takes a real load history, pasted from Excel. It counts cycles by ASTM E1049 rainflow and adds up the damage with Miner's rule.

The method follows Shigley's Mechanical Engineering Design. A full textbook problem is solved below and matches the published answers. For the theory, see the fatigue chapters of Skill-Lync's free Design of Machine Elements book.

Shigley stress-life method · ASTM E1049-85 rainflow · checked against an independent solution (7,514 checks at build) · Updated 22 Nov 2026

Material

Marin factors (Shigley)

Notch · find Kt

Mean stress and the knee

Load at the notch, nominal stress (MPa)

Stresses are nominal: the stress on the net section without the notch, as a hand calculation or a coarse FE model gives it. The calculator multiplies them by Kf. For an FE result that already includes the notch, set Kt = 1. Paste a history from Excel as one column or a comma list.

Life, Goodman2,73,208cycles · σar 236.0 MPa
Fatigue safety factor0.88n_f for infinite life
Corrected Se197.4 MPaS′e 295.0 × 0.669
Kf at the notch1.46q 0.76 · Kt 1.60
Stress with Kf160 / 189σa / σm MPa · R = 0.08
First-cycle yield1.40n_y with Kf

ka 0.761 · kb 0.879 · kc 1.00 · kd 1.000 · ke 1.000 · kf 1.00 · f 0.866 · a 1,323 MPa · b -0.1377

  • Goodman: life 2,73,208 cycles at an equivalent fully reversed amplitude of 236.0 MPa.
  • First-cycle yield (Langer): n_y = 1.40 with Kf, 2.04 on the nominal stress.
Correctionσar (MPa)n_fLife (cycles)
Goodman236.00.882,73,208
Gerber178.61.0838,51,095
Soderberg261.20.831,30,785
ASME-elliptic173.71.1156,11,693
Morrow200.90.998,78,095
SWT236.70.832,67,310
10⁰10¹10²10³10⁴10⁵10⁶10⁷10⁸200300500700cycles to failure, Nf·S = 511Se = 197S-N line (MPa, Haibach slope below the knee)your load, equivalent fully reversed (Goodman)
-20002004006000100200mean stress σm (MPa)Se 197Sy 490Sut 590GoodmanGoodman (chosen)other rulesLanger yieldload line + your load

How do you calculate fatigue life?

For a part that sees many thousands of cycles, the stress-life (S-N) method works in four steps. Start from the endurance limit of a polished test bar. Correct it for your part. Draw the S-N line. Then read your stress off it, after allowing for the notch and the mean stress.

  1. Correct the endurance limit with Marin factors for the surface finish, size, type of load, temperature and reliability. For steel the test-bar limit is about half the ultimate strength.
  2. Draw the S-N line on log-log axes, from f·Sut at 1,000 cycles to the corrected Se at a million (the knee).
  3. Find the stress at the notch. Multiply the nominal stress amplitude and mean by the fatigue notch factor Kf.
  4. Turn a mean stress into an equivalent fully reversed stress σar with a mean-stress rule, and read the life N off the line. Below Se a steel part has infinite life.

For the example shaft in the calculator (AISI 1040 cold-drawn, machined, 25 mm, rotating bending, Kt = 1.6), Se comes to 197.4 MPa. The line runs from 511 MPa at 1,000 cycles, with a = 1,323 MPa and b = -0.1377. A nominal 20 to 240 MPa stress gives σar = 236.0 MPa by Goodman, so N = 2,73,208 cycles.

f is read off a chart in Shigley. The calculator works out the same curve: Basquin's line from σ′F = Sut + 345 MPa at one reversal to 0.5 Sut at a million cycles, read at 1,000 cycles. Shigley plots it for 70 to 200 kpsi (483 to 1,379 MPa) and says to use f = 0.9 below that. Above 1,379 MPa the calculator holds the end value, 0.77, which is also what Shigley's solutions estimate for 1,600 MPa steel.

Below 1,000 cycles the part is in low-cycle fatigue and the stress-life method is not reliable. The calculator then uses Shigley's straight line from Sut at one cycle and flags the result. Use a strain-life (ε-N) method for that range.

Marin factors: surface, size, load, temperature, reliability

Shigley's 11th edition changed the surface-factor constants from those in the 10th. Many course notes and calculators still use the 10th edition's, so the calculator offers both. At Sut = 590 MPa:

Surface11th ed. a, bka (11th)10th ed. a, bka (10th)
Ground1.38, -0.0670.9001.58, -0.0850.919
Machined or cold-drawn3.04, -0.2170.7614.51, -0.2650.832
Hot-rolled38.6, -0.650.61057.7, -0.7180.591
As-forged54.9, -0.7580.436272, -0.9950.476

The size factor applies to bending and torsion only; axial loading has kb = 1. A 25 mm rotating shaft gets kb = 0.879. In a round bar that bends without rotating, only the fibres at the top and bottom reach the peak stress, so less material is highly stressed. Shigley uses an effective diameter de = 0.370 d for it. The load factor kc is 1 for bending, 0.85 for axial and 0.59 for torsion.

The temperature factor is Shigley's curve fit to tensile data for 21 steels, valid from 70 to 1,000 °F (21 to 538 °C). At 300 °C it gives kd = 0.977. Below 21 °C the calculator uses 1; low-temperature brittleness is a separate check.

The reliability factor assumes the endurance limit scatters with a standard deviation of 8% of its mean, so for a reliability with standard normal variate za:

Reliability50%90%95%99%99.9%99.99%99.999%
ke1.0000.8970.8680.8140.7530.7020.659

Shigley also lists a miscellaneous factor for things like plating, corrosion and residual stress. It has no general formula, so you type it in (kf) from your own data. For the theory and a textbook interactive on each factor, see chapter 5 of the Design of Machine Elements book.

How does a notch change fatigue life?

A fillet, groove or hole raises the local stress by the elastic factor Kt. In fatigue, real metals feel a little less than that, especially at small, sharp notches. The notch sensitivity q (0 to 1) scales it down to Kf. The calculator gets q from Neuber's equation with Shigley's fit for √a, or you can type q from a chart.

For ductile metals Shigley applies Kf to both the alternating and the mean stress, and so does this calculator. Kt for common shapes comes from the stress concentration factor calculator; the theory is in chapter 4 of the book.

Goodman, Gerber, Soderberg, ASME-elliptic, Morrow and SWT

Most parts carry a steady (mean) stress under the alternating one, and a tensile mean shortens life. The four classic rules draw a line on the mean-amplitude (Haigh) diagram from Se down to a strength on the mean axis; SWT uses the product of σmax and σa instead. Each rule turns (σa, σm) into a fully reversed amplitude σar that gives the same life, and a safety factor nf along the load line from the origin:

RuleEquivalent amplitude σarSafety factor n_f
Goodman
Gerber
Soderberg
ASME-elliptic
Morrow
Smith-Watson-Topper

Morrow needs the fatigue strength coefficient σ′f; Shigley estimates it for steel as Sut + 345 MPa. For aluminium, type a value from test data. The first-cycle yield check (Langer line) is separate:

A compressive mean. Goodman, Gerber, Soderberg and ASME-elliptic take no credit for it. Shigley sets nf = Se/σa and uses σa as σar when σm < 0, the flat line on the left of the Haigh diagram. Morrow and SWT are used as written, so they do give credit. SWT predicts no fatigue damage at all when σmax ≤ 0.

On the example shaft the six rules spread over a factor of 43 in life:

Ruleσar (MPa)n_fLife (cycles)
Goodman236.00.882,73,208
Gerber178.61.0838,51,095
Soderberg261.20.831,30,785
ASME-elliptic173.71.1156,11,693
Morrow200.90.998,78,095
SWT236.70.832,67,310

Shigley emphasises Gerber and ASME-elliptic for fatigue of ductile steel; conservative designers often use Goodman, and Soderberg is the most conservative of the four. Morrow and SWT credit a compressive mean, which the other four do not. The derivations are in chapter 6 of the book.

Worked example: a 1040 steel bar with a hole (Shigley 6-25 to 6-27)

This problem is from the Chapter 6 solutions of Shigley's Mechanical Engineering Design, 11th edition. A 25 mm wide, 10 mm thick AISI 1040 cold-drawn bar (Sut = 590 MPa, Sy = 490 MPa) has a 6 mm hole and carries an axial load. The net section is 10 × 19 mm, so 28 kN gives a nominal 147.4 MPa. Shigley takes ka = 0.76 (machined), kc = 0.85, so Se = 0.76 × 0.85 × 295 = 190.6 MPa. With Kt = 2.44 and q = 0.83, Kf = 2.20, and f = 0.87.

LoadQuantityShigleyThis calculator
±28 kN (6-25)σa with Kf324.2 MPa324.2 MPa
n_f0.590.59
Life24,613 cycles24,612 cycles
12 to 28 kN (6-26)n_f Goodman1.141.14
n_f Gerber1.421.42
n_f Morrow (σ′f = 935 MPa)1.361.36
0 to 28 kN (6-27a)n_f Goodman0.890.89
σar Goodman223.5 MPa223.5 MPa
a, b1382, −0.14341,383, -0.1434
Life329,000 cycles3,28,975 cycles
−28 to 12 kN (6-27c)n_f (compressive mean)0.820.82
Life257,000 cycles2,56,975 cycles

Every figure agrees to the digits Shigley prints, within the rounding of the solution's intermediate values. The build compares them, along with Shigley's two-level Miner problem (6-59: 7,000 cycles left at the second level). Shigley rounds ka to 0.76 and Kf to 2.20. With the unrounded values (ka = 0.761, Kf = 2.195, f = 0.866 from the chart curve) the 0 to 28 kN life is 3,37,813 cycles. A few per cent on stress moves fatigue life by tens of per cent: with b = -0.1434, life varies with about the 7th power of stress.

Rainflow counting a load history (ASTM E1049)

Real parts see irregular loads: a bracket on a vibrating engine, an axle over a rough road. To use a constant-amplitude S-N line, the history is first broken into cycles. ASTM E1049-85 (reapproved 2017) gives the standard rainflow procedure, and the calculator follows its section 5.4.4:

  1. Reduce the history to peaks and valleys. Repeated values (plateaus) and points that do not change direction are dropped.
  2. Read the points one at a time. Take X as the latest range and Y as the range before it.
  3. If X ≥ Y and Y holds the starting point, count Y as a half cycle and drop its first point. If Y does not hold it, count Y as one full cycle and drop both of its points.
  4. At the end, count every range left over (the residue) as a half cycle.

The standard's own example (Fig. 6, the history −2, 1, −3, 5, −1, 3, −4, 4, −2 units) and its count, Table X1.3, against this calculator:

RangeMeanASTM Table X1.3This calculator
90.50.50.5
800.50.5
810.50.5
610.50.5
4-10.50.5
4111
3-0.50.50.5

The verifier behind this page counts the same 31 histories two more ways: with the open-source rainflow Python package and with a four-point method written separately. The histories include repeated values and plateaus. All three agree on every cycle of every history.

Miner's rule, and what happens below the endurance limit

Each counted cycle uses up 1/N of the life, N being the life at that cycle's σar. The open question is what a cycle below Se does. On its own it never breaks a steel part. Once larger cycles have started a crack, though, small ones help it grow. The calculator gives three choices:

  • No damage below Se. Optimistic when large and small cycles mix, because the large ones lower the effective limit.
  • Extend the line below Se with the same slope. Conservative.
  • Haibach (the default): continue below Se with a flatter slope, slope factor 2k − 1, proposed by Haibach in 1970.

On the example shaft, the illustrative histories give:

Below SeBracket block: damage per passPasses to D = 1Random history: damage per passPasses to D = 1
No damage2.09 × 10⁻⁵47,8820infinite
Extend the line2.14 × 10⁻⁵46,7695.92 × 10⁻⁶1,68,785
Haibach2.13 × 10⁻⁵47,0451.38 × 10⁻⁶7,25,449

In the bracket block, the 10 large cycles do almost all the damage, so the rule hardly matters. In the random history every cycle is below Se. There the rule is the whole answer: no damage at all, or a finite life that changes about 4 times between the other two rules.

How far to trust D. Palmgren and Miner took failure at D = 1. Tests since then have put the damage sum at failure anywhere from 0.15 to 1.06. The FKM guideline asks for D = 0.3 for steel, steel castings and aluminium, and 1.0 for cast irons. Use D to compare designs or load cases, and design to the limit your code or company sets.

What this calculator does not cover

  • Low-cycle fatigue (below about 1,000 cycles, or with plastic strain every cycle): use strain-life (Coffin-Manson) with a local stress-strain model.
  • Welded joints: welds are assessed with detail-category S-N curves from codes such as Eurocode 3 or the IIW recommendations, not with Marin factors. The weld strength calculator covers the static check.
  • Multiaxial and non-proportional stresses: combine components into von Mises alternating and mean stresses first (bending with steady torsion, for example), or use a critical-plane method.
  • Surface treatments, corrosion, fretting and high temperature: shot peening, nitriding, plating and corrosive media change the endurance limit far more than the factors here. Use test data and the kf box.
  • Crack growth: once a crack is found, use fracture mechanics (Paris law) for the remaining life.
Learn durability analysis

Fatigue checks of brackets, shafts and welded frames are routine work for CAE engineers. Skill-Lync's FEA courses include fatigue analysis in SOLIDWORKS Simulation, and an S-hook fatigue project.

Frequently asked questions

How do you calculate the fatigue life of a part?

Correct the endurance limit for surface, size, load, temperature and reliability (Marin factors). Draw the S-N line from f·Sut at 1,000 cycles to Se at a million. Multiply the nominal stresses by Kf, turn the mean into an equivalent fully reversed stress with Goodman or another rule, and read the cycles off the line.

What is the formula for fatigue life?

Shigley uses Basquin's line: a straight line on log-log axes from f·Sut at 1,000 cycles to the corrected endurance limit Se at a million. The life is where your equivalent fully reversed stress σar meets that line. For the example shaft here, σar = 236.0 MPa by Goodman gives 2,73,208 cycles.

Which is better: Goodman, Gerber or Soderberg?

Shigley emphasises Gerber and ASME-elliptic for the fatigue of ductile steel, and notes that conservative designers often use Goodman. Soderberg is more conservative still, because it ends at the yield strength. On the example shaft their safety factors are 1.08, 0.88 and 0.83, so the choice changes the answer.

What is rainflow counting?

Rainflow counting turns an irregular stress history into closed cycles, each with a range and a mean, so that a constant-amplitude S-N curve can be used. ASTM E1049-85 gives the standard procedure. This calculator follows its three-point method and counts the leftover ranges (the residue) as half cycles.

What damage sum D means failure in Miner's rule?

In theory D = 1. In tests the damage sum at failure has scattered from 0.15 to 1.06, and the German FKM guideline asks designers to use D = 0.3 for steel and aluminium parts. Treat D as a way to compare designs and load histories, and keep a margin on it.

Does an aluminium alloy have an endurance limit?

No. Aluminium alloys have no fatigue limit, so tests stop at a fixed, large number of cycles. Datasheets quote the strength there: for 6061-T6, 96.5 MPa at 500 million cycles on an R.R. Moore machine. The calculator draws the S-N line to that point and continues it beyond, so it always gives a finite life.

Related on Skill-Lync

Sources

  • R.G. Budynas and J.K. Nisbett, Shigley's Mechanical Engineering Design, 11th ed., Chapter 6 solutions, Oakland University copy: surface-factor constants (ground 1.38, −0.067; machined or cold-drawn 3.04, −0.217; hot-rolled 38.6, −0.650; as-forged 12.7 kpsi, −0.758), kb = 1.24 d^−0.107, de = 0.370 d, kc, Se′ rule, Neuber √a fits, Kf on σa and σm, Goodman, Gerber and Morrow factors, σ′f = Sut + 345 MPa, n_f = Se/σa for σm < 0, Ssu = 0.67 Sut, f = 0.9 below 70 kpsi, Problems 6-25 to 6-27 and 6-59, Table A-20 strengths for AISI 1018, 1020 and 1040 CD. Read 22 Nov 2026.
  • Shigley's 10th ed. Chapter 6 solutions, Oakland University copy: eight readings of the f chart (Fig. 6-18), from 0.775 at 200 kpsi to 0.87 at 85.6 kpsi; the calculator's curve matches each within 0.005. Read 22 Nov 2026.
  • Shigley's Mechanical Engineering Design, 9th ed., pp. 277-285, University of Portland course scan: f plotted for 70 ≤ Sut ≤ 200 kpsi with Se = 0.5 Sut, the low-cycle line, the kd polynomial for 70-1000 °F, ke = 1 − 0.08 za and Table 6-5. Read 22 Nov 2026.
  • Oakland University, ME 486 equation sheet: kb = 1.51 d^−0.157 for 51 < d ≤ 254 mm, de = 0.808 √(hb), kb = 1 for axial loads. OpenExamPrep, Marin factors study guide and Engineers Edge, Marin endurance limit: the 10th-edition surface constants (1.58, 4.51, 57.7, 272). Read 22 Nov 2026.
  • University of Anbar, fluctuating stresses lecture notes (after Shigley): the Soderberg, modified Goodman, Gerber, ASME-elliptic and Langer lines and their safety-factor forms. Read 22 Nov 2026.
  • A. Ince and G. Glinka, A modification of Morrow and Smith-Watson-Topper mean stress correction models, Fatigue Fract Engng Mater Struct 34 (2011) 854: σar forms for Gerber, Goodman, Soderberg, Morrow and SWT. Read 22 Nov 2026.
  • ASTM E1049-85 (2017), Standard Practices for Cycle Counting in Fatigue Analysis, ASTM page: rainflow rules (5.4.4), the residue as half cycles, Table X1.3 for the Fig. 6 history. The history values: the rainflow R package documentation ("example from ASTM E1049-85 Fig. 6"). Read 22 Nov 2026.
  • S.A. McKelvey, Y.-L. Lee and M.E. Barkey, Stress-based uniaxial fatigue analysis using methods described in FKM-guideline, J Fail Anal Prev 12 (2012) 445: Miner-Haibach slope factor 2k − 1, critical damage sums 0.15 to 1.06, FKM D = 0.3 for steel and aluminium. Read 22 Nov 2026.
  • Aerospace Specification Metals, Aluminum 6061-T6 datasheet (ASM / Aluminum Association typical values): Sut 310 MPa, Sy 276 MPa, fatigue strength 96.5 MPa at 500,000,000 cycles, R.R. Moore. Read 22 Nov 2026.
  • Wikipedia, von Mises yield criterion: shear yield = tensile yield / √3 (0.577), used for Ssy in torsion. Read 22 Nov 2026.
  • Skill-Lync, scripts/verify/fatigue_life.py: solves the S-N line and the safety factors by bisection and counts cycles with the rainflow package and a four-point method. 82 load cases and 31 histories; the page compares 7,514 numbers with it when it is built.
Free counselling

From a fatigue hand check to a CAE career.

Durability and fatigue analysis are part of every CAE engineer's job, in SOLIDWORKS, Ansys or HyperMesh. A Skill-Lync counsellor can tell you which FEA course fits where you are now.

Talk to a CAE course counsellor

Free. We call you back, usually the same day.

By submitting you agree to our Terms and Privacy Policy.

Talk to a career counsellor

Talk to a career counsellor

Free 20-minute call. We'll map the right course to where you want to work.

By submitting you agree to our Terms and Privacy Policy.