Composite Materials cover
Interactive book · Elective (Semester 4-8)

Composite Materials

Lay up a laminate ply by ply, pull an unsymmetric one and watch it twist, fill a mould by Darcy's law and fail a laminate one ply at a time

28 chapters, 28 interactives, few words. Every chapter is mapped to the Anna University, VTU, SPPU, Mumbai University and KTU units it covers: fibres, matrices and the interface, volume fractions, hand lay-up, autoclave, RTM, pultrusion and filament winding, metal and ceramic matrix composites, micromechanics, the lamina and the angle lamina, laminate codes and the ABD matrix, ply stresses, laminate moduli, failure criteria and first-ply failure, thermal stresses, laminated plates, sandwich panels, testing, inspection and repair. The basic rule of mixtures is also in the Engineering Materials and Metallurgy book, and the filament-winding netting analysis in the Manufacturing Processes book.

  • AUCME382Composite Materials and Mechanics
  • VTUBME303Material Science and Engineering (Module 5: composites)
  • SPPU302052-AComposite Materials
  • MUMEDLO8051Composite Materials
  • KTUPEMET413Composite Materials

By Skill-Lync · Updated 20 Nov 2026 · 28 chapters · 28 interactives · free, no sign-up

Chapter 1

What a composite is: matrix, reinforcement, classification and stiffness per kilogram

Which syllabus covers thisAU CME382 Unit IVTU BME303 Module 5SPPU 302052-A Units 1, 6MU MEDLO8051 Module 1KTU PEMET413 Module 1

What makes a material a composite?

A composite combines two or more distinct materials that stay separate inside the part but work together, giving properties neither has alone. One phase, the reinforcement (fibres or particles), carries most of the load; the other, the matrix, holds it in place, shapes the part and passes load between fibres by shear. An E-glass/epoxy ply with 60 % fibre by volume has a modulus of 53.5 GPa along the fibres, sixteen times the epoxy's 3.35 GPa, but only 17.7 GPa across them. An alloy is not a composite: its phases form from one melt rather than being combined on purpose.

How are composites classified?

By matrix: polymer (PMC), metal (MMC) and ceramic (CMC). By reinforcement: particles, short fibres (random or aligned), continuous fibres (unidirectional or woven), and structural forms built from plies: laminates and sandwich panels. The form decides how stiffness varies with direction. In the interactive, E-glass/epoxy UD falls from 53.5 GPa at 0° to 22.6 GPa at 30°, a ratio of 3.38 between its stiffest and softest directions; woven 0/90 cloth narrows that to 1.97, and a [0/±45/90]s laminate gives 28.4 GPa in every direction. Short random fibres are estimated with the Tsai-Pagano average below.

What a composite is: particles, short and continuous fibres, woven cloth, laminates and sandwich, and how stiffness changes with direction: interactive loads as you scroll

Why do engineers talk about stiffness per kilogram?

For a part sized by deflection, the mass needed is proportional to density divided by modulus. Typical steel (200 GPa, 7.85 g/cm³) and 6061 aluminium (69 GPa, 2.70 g/cm³) score almost the same E/ρ, about 25.5 and 25.6 GPa per g/cm³, which is why swapping one metal for the other saves little. Unidirectional carbon/epoxy reaches 89.6. Boeing states the 787 airframe is about 50 % composites by weight. The price: cost, anisotropy, weak through-thickness strength, hidden impact damage and moisture uptake.

Are there natural, hybrid and smart composites?

Wood is cellulose fibres in a lignin and hemicellulose matrix, which is why it is much stiffer and stronger along the grain. Bone is collagen fibres stiffened by hydroxyapatite mineral crystals. A hybrid mixes two fibres in one part, for example carbon plies where stiffness matters and cheaper, tougher glass elsewhere, or carbon and aramid woven together. A smart composite carries embedded sensors or actuators, such as optical fibres that read strain or piezoelectric layers that sense and damp vibration, so the part can report its own condition.

Predict, then check

A carbon/epoxy [0/±45/90]s laminate is pulled along 0°, then a second coupon cut at 22.5° is pulled. How does the in-plane modulus change?

Worked examples

Stiffness per kilogram for a drone arm · A drone arm is sized by deflection under an axial load. Compare typical steel (200 GPa, 7.85 g/cm³), 6061-T6 aluminium (69 GPa, 2.70 g/cm³), UD carbon/epoxy T300/914C (138 GPa, 1.54 g/cm³) and the same carbon as a [0/±45/90]s laminate
  1. E/ρ steel = 200/7.85 = 25.48; aluminium = 69/2.70 = 25.56 GPa per g/cm³
  2. UD carbon/epoxy = 138/1.54 = 89.61
  3. [0/±45/90]s: own CLT gives Ex = 54.14 GPa in every direction, so E/ρ = 35.15
  4. For equal stiffness EA/L the mass scales as ρ/E: relative to steel, aluminium 0.997, quasi-isotropic carbon 0.725, UD carbon 0.284

Answer: UD carbon needs 28 % of the steel mass, the quasi-isotropic laminate 72 %; aluminium saves almost nothing

Glass beads in epoxy · Glass beads (E = 80 GPa) at Vp = 0.3 in LY556 epoxy (E = 3.35 GPa); Halpin-Tsai with ξ = 2 for spheres (illustrative filled resin)
  1. Ratio Ep/Em = 80/3.35 = 23.88; η = (23.88 − 1)/(23.88 + 2) = 0.8841
  2. E = 3.35 × (1 + 2 × 0.8841 × 0.3)/(1 − 0.8841 × 0.3) = 6.98 GPa
  3. Bounds: Reuss 1/(0.3/80 + 0.7/3.35) = 4.7 GPa, Voigt 0.3 × 80 + 0.7 × 3.35 = 26.34 GPa
  4. Density 0.3 × 2.58 + 0.7 × 1.2 = 1.614 g/cm³

Answer: E ≈ 7 GPa in every direction, about 2.1 times the resin, much nearer the lower bound

UD ply against woven cloth at 45° · E-glass/epoxy LY556 lamina: E1 = 53.48, E2 = 17.7, G12 = 5.83 GPa, ν12 = 0.278; compare a UD ply and a [0/90]s cross-ply (woven cloth without crimp) at 0° and 45°
  1. UD at 45°: 1/Ex = c⁴/E1 + (1/G12 − 2ν12/E1)s²c² + s⁴/E2 gives 16.93 GPa
  2. Cross-ply: Q11 = 54.88, Q22 = 18.16, Q12 = 5.05, Q66 = 5.83 GPa; A/h = average of the ply Q̄
  3. At 0°: Ex = 35.83 GPa; at 45° (plies at ±45): Ex = 18.21 GPa
  4. Anisotropy: UD 3.16 : 1 between 0° and 45°, cross-ply 1.97 : 1

Answer: The cloth gives up 33 % of the 0° stiffness to gain stiffness at 90°, and at 45° both are shear-dominated (16.9 and 18.2 GPa)

Chapter 2

Fibres: glass, carbon from PAN, pitch and rayon, aramid, boron, natural fibres and whiskers

Which syllabus covers thisAU CME382 Unit IVTU BME303 Module 5SPPU 302052-A Units 1, 2MU MEDLO8051 Module 1KTU PEMET413 Module 1

What is the difference between E-glass and S-glass?

Both are silica-based glasses drawn from a melt into fine filaments and coated with a sizing. E-glass, first made for electrical insulation, is the cheap workhorse of boat hulls, pipes, tanks and wind blades: about 3,445 MPa and 76 GPa at 2.58 g/cm³ (fibre values). S-2 glass, a magnesia-alumina-silica composition, reaches about 4,890 MPa and 85.5 GPa at 2.46 g/cm³: 42 % stronger and 12.5 % stiffer, at a much higher price. Glass is isotropic, so its transverse modulus equals its axial modulus.

How is carbon fibre made, and why are there so many grades?

Most carbon fibre starts as a PAN (polyacrylonitrile) precursor fibre. It is stretched and stabilised by oxidising in hot air so it will not melt, carbonised by heating in an inert gas until mostly carbon is left, optionally graphitised at a higher temperature to raise the modulus, then surface treated and sized. Pitch-based fibres reach very high modulus; rayon was the early precursor. Toray's data show the trade-off: T300 3,530 MPa and 230 GPa, T700S 4,900 MPa at the same 230 GPa, M40J 377 GPa with 4,400 MPa.

Where do aramid, boron, natural fibres and whiskers fit?

Aramid (Kevlar 49 yarn: 3,000 MPa, 112.4 GPa, 1.44 g/cm³) is light and tough in tension, which is why it stops fragments, but its fibrils buckle easily so compression strength is poor. Boron fibre is made by chemical vapour deposition of boron onto a hot tungsten wire, giving a thick, stiff fibre that is costly. Natural fibres (jute, flax, sisal, coir) are cheap and light but vary in quality and absorb moisture. Whiskers are tiny single crystals with almost no defects, hence very high strength, but hard to align.

Why is a longer fibre weaker, and a bundle weaker than its fibres?

A brittle fibre fails at its worst flaw, and a longer fibre holds more flaws. With Weibull statistics the strength scale falls as length to the power −1/m. In the interactive (σ0 = 4,000 MPa at 10 mm, m = 5, illustrative), the median strength at 100 mm is 2,345 MPa. In a bundle sharing load equally, the weak fibres break first and pass their share on: the bundle peaks at 1,498 MPa, only 0.646 of the mean single-fibre strength.

Fibres compared: strength, stiffness and density of glass, carbon and aramid, and why a longer fibre is weaker (Weibull): interactive loads as you scroll
Predict, then check

A fibre has a median strength of 4,000 MPa at 10 mm gauge length and a Weibull modulus m = 5. What median strength do you expect at 320 mm?

Worked examples

Specific strength and stiffness of four fibres · Fibre data: T700S 4,900 MPa, 230 GPa, 1.80 g/cm³; E-glass 3,445 MPa, 76 GPa, 2.58 g/cm³; Kevlar 49 3,000 MPa, 112.4 GPa, 1.44 g/cm³; steel wire 1,965 MPa, 200 GPa, 7.75 g/cm³
  1. σ/ρ (kN·m/kg): T700S 2,722, E-glass 1,335, Kevlar 49 2,083, steel wire 254
  2. E/ρ (MN·m/kg): T700S 127.8, E-glass 29.5, Kevlar 49 78.1, steel wire 25.8
  3. Against steel wire: T700S is 10.7× in σ/ρ and 5× in E/ρ; E-glass 5.3× and 1.14×

Answer: Carbon leads on both; E-glass is 5.3× steel wire in σ/ρ but only 1.14× in E/ρ, which is why glass parts are strong but flexible

Breaking load of a carbon tow · A tow of 12,000 T700S filaments (illustrative tow size), filament diameter 7 µm, fibre strength 4,900 MPa, density 1.80 g/cm³
  1. Area of one filament = π × 0.007²/4 = 38.48 × 10⁻⁶ mm²
  2. Tow area = 12,000 × that = 0.4618 mm²
  3. Breaking load = 0.4618 mm² × 4,900 MPa = 2,263 N if every filament reached the data-sheet strength
  4. Mass per km = 0.4618 mm² × 10⁶ mm × 1.80 g/cm³ ÷ 1,000 = 831 g (about 831 tex)

Answer: About 2.26 kN on a tow that weighs 0.83 g per metre; the bundle effect makes the real figure lower

Size effect and bundle strength · Weibull filament: σ0 = 4,000 MPa at L0 = 10 mm, m = 5 (illustrative); gauge length 100 mm
  1. Scale at 100 mm: σL = 4,000 × (10/100)^(1/5) = 2,524 MPa
  2. Median = σL (ln 2)^(1/5) = 2,345 MPa; mean = σL Γ(1.2) = 2,524 × 0.9182 = 2,317 MPa
  3. Equal-load-sharing bundle: maximise σ exp[−(σ/σL)^5]; the peak is at σL × 5^(−1/5) = 1,829 MPa
  4. Bundle strength = σL (5e)^(−1/5) = 1,498 MPa, 0.646 of the mean fibre strength

Answer: Median 2,345 MPa per fibre, bundle 1,498 MPa

Chapter 3

Matrices: thermosets, thermoplastics, metals and ceramics, curing and the glass transition

Which syllabus covers thisAU CME382 Unit IVTU BME303 Module 5SPPU 302052-A Unit 2MU MEDLO8051 Module 1KTU PEMET413 Module 2

What does the matrix do, and which matrices are used?

The matrix holds the fibres in position, passes load into them by shear, protects them from abrasion and moisture, supports them against buckling in compression, and largely sets the transverse and shear properties and the maximum service temperature. Epoxy LY556 has a modulus of only 3.35 GPa against 80 GPa for the glass fibre, so the transverse lamina modulus (17.7 GPa) is matrix-dominated. Polymer matrices are thermosets (epoxy, polyester, vinyl ester, phenolic) or thermoplastics (PEEK, PPS, polyamide). Metal matrices are aluminium, magnesium and titanium alloys; ceramic matrices include silicon carbide, alumina and carbon.

How does an epoxy cure, and what sets the time?

Curing links resin and hardener molecules into one network. The degree of cure α runs from 0 to 1; its rate rises steeply with temperature (Arrhenius) and is autocatalytic, so it speeds up as products form. The interactive uses a DSC-calibrated model of one epoxy. At 120 °C it gels (an infinite network forms, at α = 0.58 for an ideal stoichiometric diepoxide-diamine network) after 9.7 min and reaches α = 0.88 at 20 min; at 160 °C it gels in 1.1 min. After gelation the resin no longer flows.

Curing an epoxy: degree of cure against time and temperature, the gel point and the glass transition rising as it cures: interactive loads as you scroll

What is the glass transition, and why does a cure stall?

Below its glass transition temperature Tg a polymer is a stiff glass; above it, rubbery. As an epoxy cures its Tg climbs, here from −41.9 °C uncured to 140 °C fully cured (DiBenedetto fit). When Tg reaches the cure temperature the resin vitrifies: molecules can barely move and the reaction almost stops. Cured at 120 °C this resin stalls near α = 0.95; at 100 °C near 0.89. That is why a post-cure above the final Tg is used, and why a part should be used well below its Tg.

How is a thermoplastic matrix such as PEEK different?

A thermoplastic does not react: it is already a long-chain polymer, so a part is made by melting, shaping and cooling, in minutes rather than hours. Victrex PEEK 450G has a glass transition (onset) of 143 °C and melts at 343 °C; the data sheet lists barrel temperatures of 355 to 375 °C and a mould at 170 to 200 °C so the polymer can crystallise. It can be re-melted, welded and recycled and is tougher than epoxy, but its melt is very viscous, so wetting a dense fibre bed is hard.

Predict, then check

An epoxy whose fully cured Tg is 140 °C is held at 100 °C for 8 hours. What happens?

Worked examples

How much faster at 140 °C than at 120 °C? · Arrhenius rate constant k = A e^(−E/RT) with E = 76.6 kJ/mol (fitted for one epoxy), R = 8.31 J/(mol·K)
  1. T1 = 120 + 273.15 = 393.15 K; T2 = 140 + 273.15 = 413.15 K
  2. E/R = 76,600/8.31 = 9,218 K; 1/T1 − 1/T2 = 1.2313 × 10⁻⁴ 1/K
  3. k2/k1 = exp(9,218 × 1.2313 × 10⁻⁴) = exp(1.135) = 3.11

Answer: About 3.1 times faster: 20 °C hotter cuts the cure time to about a third

Tg during cure (DiBenedetto) · Tg0 = −41.9 °C, Tg∞ = 140 °C, λ = 0.441 (fitted values for one epoxy); find Tg at α = 0.8 and the α at which a 120 °C cure vitrifies
  1. Tg(0.8) = −41.9 + [0.441 × 0.8/(1 − 0.559 × 0.8)] × 181.9 = −41.9 + 0.6382 × 181.9 = 74.2 °C
  2. For Tg = 120 °C: y = (120 + 41.9)/181.9 = 0.89
  3. Invert y = λα/(1 − (1 − λ)α): α = y/(λ + y(1 − λ)) = 0.948

Answer: Tg = 74 °C at α = 0.8; a 120 °C cure stalls near α = 0.95

Time to gel at 120 °C · Model dα/dt = A e^(−E/RT) [(g + α)(1 − α)]^n f_d with A = 5.01 × 10⁷ 1/s, E = 76.6 kJ/mol, g = 0.352, n = 1.41, f_d the diffusion factor (bd = 4.84 K); gel point α = 1/√3 for an ideal diepoxide + diamine (amine functionality 4)
  1. Flory-Stockmayer: gel when α² (f − 1) = 1, so α_gel = 1/√3 = 0.577
  2. k(120 °C) = 5.01 × 10⁷ × exp(−76,600/(8.31 × 393.15)) = 3.291 × 10⁻³ 1/s; at α = 0 the rate is 7.551 × 10⁻⁴ 1/s
  3. Integrate with RK4 (step 0.25 s; 0.5 s gives the same answer): α reaches 0.577 at t = 585 s
  4. At 160 °C the same model gels at 67 s and passes α = 0.99 at 6.4 min

Answer: About 9.7 min at 120 °C, 1.1 min at 160 °C

Chapter 4

The interface: wetting, types of bonding and how the load gets into a fibre

Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302052-A Unit 3MU not in syllabusKTU PEMET413 Module 1

Why does the interface matter so much?

Load reaches a fibre only by shear across the interface, so the interface sets transverse and shear strength, fatigue life and moisture resistance. Too weak, and fibres slide out and the part delaminates. Too strong, and a crack in the matrix runs straight through the fibres, so the part is brittle. Polymer composites want a strong bond; ceramic matrix composites deliberately want a weak one. For a 7 µm T300 filament at 3,530 MPa held by τ = 40 MPa, the fibre is fully loaded only after 154 µm of embedded length.

What does wetting mean for a fibre and a resin?

Before any bond forms, liquid resin must spread over the fibre and push the air out. Young's equation sets the contact angle from three surface energies: cos θ = (γSV − γSL)/γLV. A resin wets a solid whose surface energy is high compared with the resin's own surface tension. In the interactive (γLV = 45, γSL = 20 mJ/m², illustrative), γSV = 40 gives θ = 63.6° and a work of adhesion Wa = γLV(1 + cos θ) = 65 mJ/m². Fibre surface treatment and sizing raise γSV; low viscosity and vacuum help the resin get in.

The fibre-matrix interface: contact angle and wetting, bonding types, and fibre pull-out against fibre break: interactive loads as you scroll

What kinds of bond form at a fibre-matrix interface?

Mechanical bonding: resin keys into a rough or etched fibre surface, strong in shear but weak in tension. Chemical bonding: a silane coupling agent on glass bonds to the glass through Si–O links at one end and reacts with the resin at the other. Reaction bonding: in metal and ceramic matrices the two phases react to form a new layer, such as a carbide when aluminium meets carbon; a thin layer helps, a thick one is brittle. Electrostatic attraction between opposite surface charges is weak. Interdiffusion: polymer chains from each side entangle, as with thermoplastic sizings.

How is interface strength measured?

In a single-fibre pull-out test the force to debond a fibre embedded a length L gives τ = F/(π d L), provided L is shorter than the critical embedded length σf d/(4τ), otherwise the fibre breaks first. The microbond test does the same with a resin droplet. In the fragmentation test one fibre in a resin coupon is stretched until it stops breaking; Kelly-Tyson gives τ = σf d/(2 lc), with lc about 4/3 of the mean fragment length. The simulation at τ = 40 MPa estimates 49 MPa: weak spots break early, so the 4/3 rule over-estimates.

Predict, then check

The interface shear strength of a fibre-matrix pair is doubled by a better sizing. What happens to the critical embedded length, beyond which the fibre breaks instead of pulling out?

Worked examples

Contact angle before and after surface treatment · Resin surface tension γLV = 42 mJ/m², solid-liquid energy γSL = 15 mJ/m²; treated fibre γSV = 50 mJ/m², untreated 30 mJ/m² (illustrative values)
  1. Treated: cos θ = (50 − 15)/42 = 0.8333, θ = 33.6°
  2. Work of adhesion Wa = 42 × (1 + 0.8333) = 77 mJ/m² (= γSV + γLV − γSL = 50 + 42 − 15)
  3. Untreated: cos θ = (30 − 15)/42 = 0.3571, θ = 69.1°, Wa = 57 mJ/m²

Answer: Treatment cuts the contact angle from 69° to 34° and raises Wa by 35 %

Critical embedded length of a glass fibre · E-glass fibre d = 14 µm (illustrative), strength 3,445 MPa, interface shear strength τ = 35 MPa (uniform along the embedded length, an assumption); embedded length 200 µm
  1. Fibre break load = 3,445 × π × 0.014²/4 = 0.53 N
  2. Debond load at L = 0.2 mm: π × 0.014 × 0.2 × 35 = 0.308 N, smaller, so the fibre pulls out
  3. Critical embedded length L = σf d/(4τ) = 3,445 × 14/(4 × 35) = 344.5 µm
  4. Check: π × 0.014 × 0.3445 × 35 = 0.53 N = break load

Answer: It pulls out at 0.31 N; beyond 344 µm embedded it would break at 0.53 N

Interface strength from a fragmentation test · A carbon fibre, d = 7 µm, in an epoxy coupon stretched to saturation; mean fragment length 0.30 mm (illustrative measurement); fibre strength at the critical length taken as 3,530 MPa
  1. Critical length lc ≈ (4/3) × 0.30 = 0.4 mm (fragments assumed spread evenly between lc/2 = 0.2 and lc = 0.4 mm)
  2. Kelly-Tyson: τ = σf d/(2 lc) = 3,530 × 0.007/(2 × 0.4) = 30.9 MPa
  3. Caveat: the fibre strength at so short a length is higher than the data-sheet value (Weibull), which would raise τ

Answer: τ ≈ 31 MPa

Chapter 5

Volume fraction, weight fraction, density and void content

Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302052-A Unit 4MU MEDLO8051 Module 4KTU not in syllabus

Why does the fibre volume fraction matter so much?

Along the fibres a lamina is roughly a weighted average of fibre and matrix, so its stiffness and strength rise almost in proportion to the fibre volume fraction Vf. With T300 carbon (230 GPa) in 914C epoxy (4.0 GPa), going from Vf = 0.50 to 0.60 lifts E1 from 117 to 139.6 GPa, 19 % more; the measured T300/914C lamina at Vf 0.6 is 138 GPa. Mass barely changes, so every extra point of Vf is nearly free stiffness. The basic rule of mixtures is also in the Engineering Materials and Metallurgy book.

How high can the fibre volume fraction go?

Picture the fibres as circles on a grid. On a square grid with centre spacing s and diameter d, Vf = π/(4(s/d)²); on a hexagonal grid the factor is π/(2√3). Touching fibres set the ceilings: 0.785 square and 0.907 hexagonal. At s/d = 1.15, the interactive's start, the square array holds 0.594 and the hexagonal 0.686, and with 7 µm fibres the resin gap is only about 1.05 µm. Real laminates sit well below these limits: fibres wander and touch at random, and resin has to flow between them.

Fibre volume fraction: square and hexagonal packing limits, weight to volume fraction and the void content from density: interactive loads as you scroll

Why convert between weight and volume fraction?

Prepregs and burn-off tests are measured by weight, but stiffness models need volume. Divide each mass by its density: Vf = (Wf/ρf)/(Wf/ρf + Wm/ρm). Hexcel's 8552/35%/134 prepreg is 35 % resin by weight. With AS4 fibre at 1.79 g/cm³ and resin at 1.30 g/cm³, that gives Vf = 57.42 %, density 1.581 g/cm³ and a 0.130 mm cured ply for 134 g/m² of fibre, matching the datasheet's 57.42 %, 1.58 g/cm³ and 0.130 mm. Carbon is denser than epoxy, so the weight fraction always reads higher than the volume fraction.

How is void content measured, and why does 1 % matter?

ASTM D2734 burns off or digests the resin to get the weight fractions. It works out the theoretical density Td = 1/(Wf/ρf + Wm/ρm) and compares it with the measured density Md from weighing in air and water: voids = (Td − Md)/Td. A good laminate has about 1 % voids or less. Voids lower fatigue life, let water in and widen the scatter in strength. For AS4/8552 at 65 % fibre by weight, Td = 1.581 g/cm³, so a coupon measuring 1.558 g/cm³ holds 1.5 % voids.

Predict, then check

Laminate A is 65 % carbon fibre by weight; laminate B is 65 % carbon fibre by volume, same fibre and epoxy. Which has more fibre in it?

Worked examples

Void content of a glass/epoxy coupon from a burn-off test · A coupon weighs 4 g in air and 1.945 g in water (0.997 g/cm³). After burning off the resin, 2.92 g of glass remains. E-glass 2.58 g/cm³, epoxy 1.20 g/cm³ (illustrative coupon and epoxy density).
  1. Fibre weight fraction Wf = 2.92/4 = 0.73
  2. Measured density Md = 4 × 0.997/(4 − 1.945) = 1.9406 g/cm³
  3. Theoretical density Td = 1/(0.73/2.58 + 0.27/1.20) = 1.9687 g/cm³
  4. Voids = (1.9687 − 1.9406)/1.9687 = 1.43 %
  5. Check by mass balance: Vf = Wf·Md/ρf = 0.5491, Vm = (1 − Wf)·Md/ρm = 0.4366, so voids = 1 − 0.5491 − 0.4366 = 1.43 %

Answer: Vf = 0.549, voids ≈ 1.4 %: above the 1 % mark for good laminates

Ply thickness and ply count for a drone arm · A T300 woven prepreg has 200 g/m² of fibre and 38 % resin by weight. T300 is 1.76 g/cm³ and the epoxy 1.20 g/cm³ (illustrative). The tube wall must be at least 3.0 mm.
  1. Wf = 0.62 → Vf = (0.62/1.76)/(0.62/1.76 + 0.38/1.20) = 0.5266
  2. Fibre volume per m² = 200 g / 1.76 g/cm³ = 113.64 cm³, a solid fibre layer 0.1136 mm thick
  3. Cured ply t = 0.1136/0.5266 = 0.2158 mm
  4. Plies for 3.0 mm: 3.0/0.2158 = 13.9 → 14 plies (3.02 mm)
  5. Laminate density = 0.5266 × 1.76 + 0.4734 × 1.20 = 1.495 g/cm³

Answer: t = 0.216 mm per ply, 14 plies, Vf = 0.527

Packing limit with a thin resin gap · 7 µm carbon fibres with a 0.5 µm resin layer between neighbours, so the centre spacing is 7.5 µm
  1. s/d = 7.5/7 = 1.0714
  2. Square array: Vf = π/(4 × 1.0714²) = 0.6842
  3. Hexagonal array: Vf = π/(2√3 × 1.0714²) = 0.79
  4. A hexagonal array at Vf = 0.60 needs s/d = √(0.9069/0.60) = 1.2294, a gap of 1.61 µm

Answer: Square 0.684, hexagonal 0.79; a 60 % laminate leaves about 1.6 µm of resin between fibres

Chapter 6

Hand lay-up, spray-up, vacuum bagging and autoclave curing of prepregs

Which syllabus covers thisAU CME382 Unit IVTU not in syllabusSPPU 302052-A Unit 2MU MEDLO8051 Module 1KTU PEMET413 Module 2

How do hand lay-up and spray-up work, and what limits them?

Both use one open mould. It is waxed with release agent and sprayed with a gelcoat that becomes the finished surface. In hand lay-up, glass mat or fabric is laid in, wetted with resin and pressed with a roller. In spray-up, a gun chops roving and sprays it with catalysed resin. Tooling is cheap, so a Hosur shop can make a few bus panels from one mould. The catch: the only pressure is the roller (close to 0 bar), so fibre content stays low, voids and thickness depend on the worker, and only one face is smooth.

What does each layer of a vacuum bag do?

Bottom up: the tool; a release film so the part lets go; the prepreg plies; a peel ply that is torn off later to leave a clean surface for bonding; a perforated release film that lets air and a little resin through; a breather that keeps a path open to the port; then the bag, sealed with tape to the tool, with a vacuum port. Pump the air out and the atmosphere presses on the bag with at most 1 atm, 1.013 bar. That is about 10.3 tonnes on every square metre.

Vacuum bagging layer by layer, hand lay-up to autoclave, and a prepreg cure cycle of temperature and pressure: interactive loads as you scroll

What does an autoclave add?

An autoclave is a heated pressure vessel. It adds gas pressure on top of the vacuum. The Hexcel 8552 datasheet asks for full vacuum and 7 bar gauge for solid laminates. Once the vessel reaches about 1 bar, the vacuum is cut to a 0.2 bar safety value, so the part feels about 7.2 bar, against at most 1 bar from a bag alone. The pressure squeezes out trapped air, keeps volatiles dissolved and packs the plies to the nominal 0.130 mm. Honeycomb sandwich parts get only 3.2 bar, so the core is not crushed.

Why does a prepreg cure cycle have two holds?

8552 is heated at 1-3 °C/min to 110 °C and held for 60 minutes. Its viscosity is low there, so resin flows, wets the fibres and lets air escape before the gel point. Then it is heated at 1-3 °C/min to 180 °C and held for 120 minutes to cure. It cools at 2-5 °C/min and is vented at 60 °C or below. Starting at 20 °C, with 2 °C/min up and 3 °C/min down, the cycle takes 300 minutes. Thick parts need the slower rates, so the inside keeps up with the thermocouples.

Predict, then check

A vacuum bag at sea level is pumped to a perfect vacuum. What is the most pressure the atmosphere can put on the laminate?

Worked examples

How long is the 8552 cycle at the slowest and fastest rates? · Hexcel 8552 monolithic cycle from 25 °C: up to 110 °C (hold 60 min), up to 180 °C (hold 120 min), cool to 60 °C. Heating 1-3 °C/min, cooling 2-5 °C/min.
  1. Slowest: 85 + 60 + 70 + 120 + 60 = 395 min
  2. Fastest: 28.3 + 60 + 23.3 + 120 + 24 = 255.7 min
  3. The two holds alone take 180 min, 70 % of the fastest cycle

Answer: 4.26 h to 6.58 h of autoclave time per load

Force on a spar-cap panel: bag against autoclave · A 1.2 m × 0.8 m carbon spar-cap panel. The bag gauge reads −0.95 bar in an oven. In the autoclave it is 7 bar gauge with the vacuum cut to 0.2 bar (illustrative panel).
  1. Area = 1.2 × 0.8 = 0.96 m²
  2. Bag only: 0.95 bar = 95 kPa, force = 95,000 × 0.96 = 91.2 kN
  3. Autoclave: 7 + 0.2 = 7.2 bar, force = 720,000 × 0.96 = 691 kN
  4. Ratio = 7.2/0.95 = 7.58

Answer: 91 kN from the bag, 691 kN in the autoclave, 7.6 times more squeeze

What bagging does to a chopped-mat laminate · 4 layers of 450 g/m² E-glass chopped strand mat (2.58 g/cm³) in epoxy (1.20 g/cm³). Hand-rolled to 30 % glass by weight, or vacuum-bagged to 40 % (illustrative fractions).
  1. Glass per m² = 4 × 450 = 1,800 g
  2. Hand lay-up: Vf = 0.1662, thickness = 1,800/(2,580 × 0.1662) = 4.2 mm, resin 4,200 g/m²
  3. Vacuum bag: Vf = 0.2367, thickness = 1,800/(2,580 × 0.2367) = 2.95 mm, resin 2,700 g/m²
  4. Same glass, 30 % thinner and 1,500 g lighter per m²

Answer: 4.2 mm → 2.95 mm; Vf 0.17 → 0.24

Chapter 7

Closed moulding: RTM, vacuum infusion, compression moulding (SMC/BMC) and reinforced injection moulding

Which syllabus covers thisAU CME382 Unit IVTU not in syllabusSPPU 302052-A Unit 2MU MEDLO8051 Module 1KTU not in syllabus

What are the main closed-mould processes?

Resin transfer moulding (RTM) puts a dry fibre preform in a matched two-part mould and pumps resin in; Hexcel quotes atmospheric to 5 bar for its RTM6 resin. Vacuum infusion uses one mould and a bag, and the vacuum (below 5 mbar) pulls resin through. Compression moulding presses sheet or bulk moulding compound (SMC, BMC: resin, filler and chopped glass) in hot steel dies. Reinforced injection and reaction injection moulding (RRIM) shoot short-fibre material into a closed mould. Both faces come out finished and the styrene stays inside.

How long does a mould take to fill?

Resin creeping through fibres obeys Darcy's law: flow speed = (K/μ) × pressure gradient, where K is the permeability. With a line gate and constant pressure, the gradient falls as the front moves away, so the front slows: x grows as √t and the fill time grows as L². With the interactive's defaults (3 bar, 100 mPa·s, Vf 0.45, 0.4 m, K = 8.24×10⁻¹² m²), RTM fills in 29.6 min. Infusion at 0.95 bar takes 93.6 min, and the resin must stay runny that long.

Resin transfer moulding and vacuum infusion: Darcy's law, the flow front through the fibres and the fill time: interactive loads as you scroll

What sets the permeability of a preform?

The Kozeny-Carman model treats the gaps between fibres as tiny pipes: K = r²(1 − Vf)³/(4kVf²), with r the fibre radius and k the Kozeny constant. Both the r² and the (1 − Vf)³ hit hard. Raising Vf from 0.45 to 0.55 cuts K by a factor of 2.73. Here k = 1.8 and a 17 µm glass filament are illustrative, and research shows k is not really constant. Woven fabrics fill faster than this through the larger gaps between tows, which is why moulders measure K for every new fabric.

Why are gate and vent positions so important?

A point gate is the slowest choice. Resin spreads out in a circle, so the same pressure drives an ever longer front. Filling 0.4 m from a 5 mm gate takes 115 min, against 29.6 min from a line gate along one edge. Moulders therefore feed resin along runners or a flow mesh and put vents at the last point to fill. Resin that races along a gap at the mould edge can surround a dry patch, and that patch is scrap.

Predict, then check

An RTM mould is made twice as long, with the same fabric, resin and injection pressure. The fill time becomes:

Worked examples

RTM fill time of a bus-front panel · Glass preform at Vf = 0.40, flow length 0.8 m from a line gate, ΔP = 4 bar, μ = 0.15 Pa·s. K from Kozeny-Carman with r = 8.5 µm and k = 1.8 (illustrative).
  1. K = (8.5×10⁻⁶)² × 0.6³/(4 × 1.8 × 0.40²) = 13.55×10⁻¹² m²
  2. φ = 1 − 0.40 = 0.60
  3. t = 0.15 × 0.60 × 0.8²/(2 × 13.55×10⁻¹² × 4×10⁵) = 5,315 s = 88.6 min
  4. Front speed at the vent = KΔP/(μφL) = 0.075 mm/s

Answer: 88.6 min (about 1.5 h): the resin must stay runny for longer than that

Infusion instead, and the pressure for a 20-minute fill · The same panel by vacuum infusion at ΔP = 0.95 bar; then by RTM with a target fill time of 20 min
  1. Infusion: t = 88.6 min × 4/0.95 = 373 min
  2. For t = 1,200 s: ΔP = μφL²/(2Kt)
  3. ΔP = 0.15 × 0.60 × 0.64/(2 × 13.55×10⁻¹² × 1,200) = 17.72 bar

Answer: Infusion 373 min; RTM needs 17.7 bar for 20 min, more than the 5 bar ceiling, so add gates instead

Point gate against line gate · The same preform (K and φ as in Example 1), ΔP = 4 bar, μ = 0.15 Pa·s; fill 0.3 m from a line gate, or 0.3 m radius from a 5 mm point gate
  1. Line gate: t = 0.15 × 0.60 × 0.3²/(2KΔP) = 12.46 min
  2. Point gate: t = μφ/(4KΔP) × [R²(2 ln(R/R0) − 1) + R0²]
  3. Bracket = 0.09 × (2 ln 60 − 1) + 0.000025 = 0.647 m²
  4. t = 0.15 × 0.60/(4 × 13.55×10⁻¹² × 4×10⁵) × 0.647 = 44.8 min

Answer: 12.5 min against 44.8 min: the point gate is 3.6 times slower

Chapter 8

Pultrusion and filament winding: line speed, cure in the die and winding patterns

Which syllabus covers thisAU CME382 Unit IVTU not in syllabusSPPU 302052-A Unit 2MU MEDLO8051 Module 1KTU PEMET413 Module 2

How does pultrusion make a profile?

Rovings and mats are pulled off a creel and through a resin bath (polyester, vinylester, polyurethane or epoxy). A preformer gathers them into shape, and they pass through a heated steel die where the resin cures. Pullers grip the hard profile and a flying saw cuts it to length. A 1981 patent describes dies of 3-5 ft (0.91-1.52 m) in four heated zones, with a one-inch rod speeded up from 3 to 6 ft/min (0.91 to 1.83 m/min). The output is continuous, constant-section profiles such as gratings, cable trays and ladder rails.

What limits the line speed of a pultrusion line?

The resin must cure before it leaves the die. Material spends L/v in a die of length L at speed v. With first-order cure, the degree of cure at the exit is 1 − e^(−kL/v), where k rises steeply with die temperature. With the interactive's illustrative resin (k = 0.05 /s at 160 °C), a 0.9 m die at 1 m/min gives 54 s and 0.933 cure. At 2.5 m/min the cure drops to 0.66, so the profile would come out soft. For 90 % cure the limit is 1.17 m/min. A longer or hotter die buys speed.

Pultrusion line speed against cure in the die, and hoop, helical and polar winding patterns on a mandrel: interactive loads as you scroll

What are hoop, helical and polar winding?

The winding angle α is measured from the mandrel axis. Hoop winding lays the band almost round the mandrel. The carriage moves one band width per turn, so cos α = b/(πD): 88.9° for a 12 mm band on a 200 mm mandrel. Helical winding runs the band to and fro at a chosen angle in between and turns it around at the ends. Polar winding sweeps the band in a flat plane past the two end openings of a vessel at a small angle. Choosing the angle from the pressure loads (netting analysis) is in the Manufacturing Processes book.

How many circuits does it take to cover a mandrel?

Unroll the mandrel. A band of width b at angle α crosses the circumference over b/cos α, so one closed ±α layer takes n = πD cos α/b circuits, rounded up. Each turn of the mandrel the band also advances the lead πD/tan α along the axis. For D = 200 mm, b = 12 mm and α = 45°, n = 37.02, rounded up to 38, and the lead is 628 mm. At 60° only 26.2 circuits are needed, against 45.3 at 30°. A dome with an end opening one third of the radius allows a geodesic angle of 19.5° (R sin α = r0).

Predict, then check

On the same mandrel with the same band, the helical winding angle goes from 30° to 60°. How many circuits does one full layer take?

Worked examples

Line speed of a pultruded rod · A 1.2 m die at 170 °C. Illustrative first-order cure: Ea = 60 kJ/mol, k = 0.05 /s at 160 °C. Find the fastest speed for 90 % and for 95 % cure at the exit.
  1. k(170 °C) = 0.05 × exp[−(60,000/8.314)(1/443.15 − 1/433.15)] = 0.0728 /s
  2. For 90 %: v = 60kL/ln 10 = 60 × 0.0728 × 1.2/2.3026 = 2.277 m/min
  3. For 95 %: v = 60kL/ln 20 = 60 × 0.0728 × 1.2/2.9957 = 1.75 m/min
  4. Check: residence at 1.75 m/min = 41.1 s; 1 − e^(−0.0728 × 41.1) = 0.95

Answer: 2.28 m/min for 90 %, 1.75 m/min for 95 % cure

Helical pattern on an FRP pipe · Mandrel D = 300 mm, band b = 15 mm, winding angle 55° (illustrative pipe)
  1. Band width around the circumference = 15/cos 55° = 26.15 mm
  2. Circumference = π × 300 = 942.5 mm
  3. Circuits n = 942.5/26.15 = 36.04 → 37 circuits for one closed ±55° layer
  4. Lead per turn = π × 300/tan 55° = 660 mm
  5. Counting bands of 26.15 mm spaced evenly round 942.5 mm: 37 is the first count that leaves no gap

Answer: 37 circuits, lead 660 mm

Time for a hoop layer · The same pipe, 1.5 m long; hoop layer with the same 15 mm band; mandrel at 20 rpm (illustrative)
  1. Hoop angle: cos α = 15/(π × 300) → α = 89.09°
  2. Axial advance per turn = 15/sin α = 15.002 mm
  3. Turns = 1,500/15.002 ≈ 100
  4. Time = 100/20 = 5 min

Answer: α ≈ 89.1°, 100 turns, about 5 min per hoop layer

Chapter 9

Metal matrix composites: matrices, particles and fibres, and the properties they give

Which syllabus covers thisAU CME382 Unit IVTU BME303 Module 5SPPU 302052-A Unit 3MU not in syllabusKTU PEMET413 Module 3

What is a metal matrix composite, and why make one?

A metal matrix composite (MMC) is a light metal, usually aluminium, magnesium or titanium, filled with a stiff ceramic: particles of SiC or Al₂O₃, short whiskers, or continuous fibres. The metal keeps its toughness and conductivity; the ceramic adds stiffness, wear resistance and a lower thermal expansion. Compared with a polymer composite an MMC works hotter, conducts heat and does not absorb moisture. AlSiC, aluminium with 37 to 63 vol% SiC, is made by pushing molten aluminium into a SiC preform and is used as a base plate for power electronics. At 63 vol% the mixture rule gives 3.02 g/cm³ (6061 matrix); the grade's listed density is 3.01.

Why can you only bound the modulus of a particle composite?

The modulus depends on how the particles are arranged, not only on how much there is. If both phases strain alike (Voigt) you get the upper limit, if both carry the same stress (Reuss) the lower. For 20 vol% SiC in Al 6061 these are 138.1 and 82.7 GPa, far apart. Hashin and Shtrikman found the tightest bounds for any isotropic two-phase mix: 92.7 to 115 GPa. Halpin-Tsai with ξ = 2 for equiaxed particles gives 98.5 GPa, near the lower bound, where real particle composites usually sit. Slide ξ: 0 gives Reuss, a very large ξ gives Voigt.

Particle-reinforced aluminium: modulus between the Voigt, Reuss and Hashin-Shtrikman bounds, and the thermal expansion: interactive loads as you scroll

Why does SiC cut the expansion of aluminium more than the rule of mixtures predicts?

Heated together, the aluminium wants to grow 23.6 millionths per °C and the SiC only 4.4. The stiff particles hold the aluminium back, so the composite expands less than a volume average. Turner's equation weights each phase's expansion by its bulk modulus K times its volume fraction: at 20 vol% SiC it gives 15.4 × 10⁻⁶/°C against 19.8 from the plain mixture rule. Levin's exact relation puts the truth between the two; the shaded band uses the Hashin-Shtrikman bulk moduli. That is why a high-SiC aluminium can be matched to ceramic circuit boards and chips. Al₂O₃ particles, which expand more (7.1) but are even stiffer in bulk, give 15.6 at the same fraction.

What do you give up with an MMC?

Stiffness per kilogram goes up: at 20 vol% SiC the specific modulus is about 1.45 times that of aluminium. The price is ductility and toughness, since cracks start at particle clusters and broken particles. The hard SiC wears out ordinary cutting tools, so parts are cast or forged close to shape and machined with diamond tools. Held too hot or too long, molten aluminium reacts with SiC to form brittle aluminium carbide at the interface. And the material costs more than the plain alloy, so MMCs appear where stiffness, wear or expansion matter, such as brake parts and electronics base plates.

Predict, then check

Aluminium (23.6 × 10⁻⁶/°C) gets 30 vol% SiC (4.4 × 10⁻⁶/°C). The composite's expansion coefficient is:

Worked examples

Modulus bounds for a 30 % SiC brake disc alloy · A Hosur foundry trials Al 6061 with 30 vol% SiC particles for a two-wheeler brake disc (illustrative). Al: E 68.9 GPa, ν 0.33. SiC: K 203 GPa, G 179 GPa.
  1. Aluminium: K = E/(3(1 − 2ν)) = 67.55 GPa, G = E/(2(1 + ν)) = 25.9 GPa; SiC: E = 9KG/(3K + G) = 415 GPa
  2. Voigt: 0.3 × 415 + 0.7 × 68.9 = 172.7 GPa; Reuss: 1/(0.3/415 + 0.7/68.9) = 91.9 GPa
  3. HS lower bound (aluminium as the reference): K = 88.6 GPa, G = 41.6 GPa, so E = 9KG/(3K + G) = 107.8 GPa
  4. HS upper bound (SiC as the reference): K = 98.6 GPa, G = 55.8 GPa, so E = 140.8 GPa
  5. Halpin-Tsai, ξ = 2: η = (6.023 − 1)/(6.023 + 2) = 0.6261, E = 116.7 GPa, inside the HS band

Answer: E lies between 108 and 141 GPa (Halpin-Tsai 117 GPa), against 68.9 GPa for the alloy

An AlSiC electronics base plate · A power-module base plate needs 63 vol% SiC in aluminium (the AlSiC-9 recipe). Use Al 6061 values: 2.70 g/cm³, 23.6 × 10⁻⁶/°C, K 67.55 GPa; SiC 3.21 g/cm³, 4.4 × 10⁻⁶/°C, K 203 GPa.
  1. Density: 0.63 × 3.21 + 0.37 × 2.70 = 3.021 g/cm³ (AlSiC-9 with A356 alloy is listed at 3.01)
  2. Rule of mixtures CTE: 0.63 × 4.4 + 0.37 × 23.6 = 11.5 × 10⁻⁶/°C
  3. Turner: (4.4 × 203 × 0.63 + 23.6 × 67.55 × 0.37)/(203 × 0.63 + 67.55 × 0.37) = 7.54 × 10⁻⁶/°C
  4. Levin's exact two-phase relation α = αm + (αp − αm)(1/K − 1/Km)/(1/Kp − 1/Km) gives the mixture rule with the Reuss K and Turner with the Voigt K, so these two bracket the truth
  5. With the tighter HS bulk-modulus bounds (124.8 to 140.9 GPa) Levin narrows the range to 8.62 to 10.4 × 10⁻⁶/°C

Answer: ρ ≈ 3.02 g/cm³, α ≈ 8.6 to 10.4 × 10⁻⁶/°C, close to ceramics and far below aluminium's 23.6

How much SiC for 50 % more stiffness per kilogram? · Find the SiC fraction at which E/ρ of Al-SiC reaches 1.5 times that of aluminium (68.9/2.70 = 25.5 GPa per g/cm³), using the cautious HS lower bound.
  1. Target: 1.5 × 25.52 = 38.28 GPa per g/cm³
  2. E/ρ on the HS lower bound rises with Vp; bisection between 0 and 1 converges at Vp = 0.31
  3. Check: E = 109.4 GPa, ρ = 2.858 g/cm³, E/ρ = 38.28
  4. On the HS upper bound the same gain needs only Vp = 0.166: the arrangement of the particles matters

Answer: About 31 vol% SiC (lower-bound estimate; 17 vol% if the particles behaved like the upper bound)

Chapter 10

Making MMCs: stir casting, squeeze casting, pressure infiltration, powder metallurgy and diffusion bonding

Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302052-A Unit 3MU MEDLO8051 Module 1KTU PEMET413 Module 3

What are the main ways of making a metal matrix composite?

Liquid-state routes mix the ceramic with molten metal: stir casting (particles stirred into the melt, then cast), squeeze casting and pressure infiltration (melt forced into a porous preform of particles or fibres), spray deposition and in-situ reaction, where the reinforcement forms inside the melt. They are cheap and make large castings. Solid-state routes avoid melting: powder metallurgy blends metal and ceramic powders, compacts and sinters or hot-presses them, and diffusion bonding presses metal foils and fibre mats together under heat. They give even particle spread and avoid melt reactions, at a higher cost.

Why do particles settle in stir casting, and what controls it?

SiC (3.21 g/cm³) is denser than molten aluminium (2.375), so once the stirrer stops each particle sinks at the Stokes speed. With the melt at about 1.3 mPa·s, a 20 µm particle falls 0.14 mm/s: 42 mm of particle-free melt forms at the top in 5 minutes. Speed grows with the square of size, so 100 µm particles fall 3.5 mm/s, still slow enough for Stokes' law (Reynolds number 0.64, below 1). Pour soon after stirring, or stir a semi-solid slurry: at about 300 mPa·s settling is 231 times slower.

Stir casting particles into molten aluminium: Stokes settling, and the pressure needed to infiltrate a preform: interactive loads as you scroll

Why does molten aluminium need pressure to enter a preform?

Liquid aluminium does not wet SiC or carbon well: its contact angle is about 150°, so surface tension pushes the melt out of narrow pores. The melt enters only above a threshold pressure equal to the surface tension times |cos θ| times the pore surface per unit pore volume, 6Vp/((1 − Vp)d) for packed particles. For 20 µm SiC at 55 vol%, with γ = 0.8 N/m, that is 0.25 MPa, about 2.5 atmospheres, more than a vacuum bag can give. At 5 µm it rises to 1.02 MPa. Squeeze casting presses far harder and holds the pressure while the metal freezes.

How do powder metallurgy and diffusion bonding work?

In powder metallurgy, aluminium and SiC powders are weighed out, blended, cold-pressed in a die, degassed and sintered or hot-pressed, then usually extruded or forged to close the last pores and break up particle clusters. For 20 vol% SiC the blend is 22.9 % SiC by weight, because SiC is denser. Diffusion bonding builds continuous-fibre MMCs: layers of fibre mat alternate with thin metal foils, and the stack is pressed hot in vacuum, below the melting point, until the foils flow round the fibres and bond.

Predict, then check

A foundry halves its SiC particle size from 40 µm to 20 µm. How fast do the new particles settle in the melt?

Worked examples

Settling while the ladle waits · Al-10 vol% SiC melt, particles 30 µm, held 2 minutes in a 120 mm deep ladle before pouring (illustrative). ρ SiC 3210 kg/m³, melt 2375 kg/m³, μ 1.3 mPa·s.
  1. v = (3210 − 2375) × 9.81 × (30 × 10⁻⁶)²/(18 × 1.3 × 10⁻³) = 0.315 mm/s
  2. Reynolds number = 2375 × 0.0003151 × 30 × 10⁻⁶/(1.3 × 10⁻³) = 0.0173, far below 1: Stokes' law holds
  3. Clear layer after 120 s = 0.315 × 120 = 37.8 mm, 32 % of the depth
  4. Those particles pack at 0.6 at the bottom: sediment = 37.8 × 0.1/0.6 = 6.3 mm

Answer: The top 38 mm loses its SiC and about 6 mm of sediment builds up; pour sooner or keep stirring

Threshold pressure for two preforms · (a) SiC particles 10 µm at Vp 0.5; (b) carbon fibres 7 µm at Vf 0.45. Liquid Al: γ = 0.8 N/m, θ = 150°.
  1. (a) Pore surface per pore volume S = 6 × 0.5/((1 − 0.5) × 10 × 10⁻⁶) = 0.6 × 10⁶ per m
  2. (a) P0 = S × γ × |cos 150°| = 0.6 × 10⁶ × 0.8 × 0.866 = 0.416 MPa
  3. (b) Fibres: S = 4 × 0.45/(0.55 × 7 × 10⁻⁶), P0 = 0.324 MPa
  4. Both exceed 1 atm (0.101 MPa): (a) by 4.1 times, so pressure must be applied

Answer: (a) 0.42 MPa, (b) 0.32 MPa just to start; viscous drag and freezing demand more (Ma's carbon preform filled at 7 MPa, not at 3.5)

Weighing a powder-metallurgy batch · A 5 kg batch of Al with 15 vol% SiC by powder metallurgy (Al 2.70, SiC 3.21 g/cm³, no porosity).
  1. Weight fraction of SiC = 0.15 × 3.21/(0.15 × 3.21 + 0.85 × 2.70) = 0.1734
  2. SiC powder = 5 × 0.1734 = 0.867 kg; aluminium powder = 4.133 kg
  3. Composite density = 0.15 × 3.21 + 0.85 × 2.70 = 2.7765 g/cm³, so the batch makes 1801 cm³ of fully dense billet

Answer: 0.87 kg SiC + 4.13 kg Al (17.3 wt% SiC)

Chapter 11

Ceramic matrix composites: how fibres make a brittle ceramic tough

Which syllabus covers thisAU CME382 Unit IVTU BME303 Module 5SPPU not in syllabusMU not in syllabusKTU PEMET413 Module 4

Why put fibres in a ceramic at all?

Ceramics such as SiC and alumina keep their strength far above the melting point of aluminium and resist wear and oxidation, but they are brittle: a monolithic ceramic breaks at about 0.05 to 0.10 % strain with no warning, and one flaw is enough. Continuous fibres change that. A ceramic matrix composite (CMC) can stretch up to about 1 % before failure, and it cracks gradually instead of shattering. That is why C/SiC brake discs, which weigh about 40 % of a metal disc, and SiC/SiC turbine shrouds and combustor liners exist. The aim is toughness, not extra stiffness.

What decides whether a matrix crack is stopped at a fibre?

A crack running through the matrix reaches a fibre and has two choices: cut straight through the fibre, or turn and run along the fibre-matrix interface. He and Hutchinson showed that when the fibre and matrix have similar stiffness the crack turns if the interface's fracture energy Gi is below about a quarter of the fibre's Gf. A crack kinked through 90° releases only one quarter of the energy of a straight one, which is where the 1/4 comes from. Designers therefore coat fibres with a deliberately weak interphase, pyrolytic carbon or boron nitride. Move the Gi/Gf slider past 0.25 and the CMC turns brittle.

Ceramic matrix composites: brittle against graceful failure, crack deflection at a weak interface and fibre bridging: interactive loads as you scroll

How do bridging and pull-out make a CMC tough?

Once the crack has turned, the fibres stay whole across it and hold it shut (bridging), so the load can keep rising after the matrix has cracked. When fibres finally break, at weak points away from the crack plane, they must be pulled out of their sockets against the interface sliding stress τ, which soaks up more energy. In the illustrative coupon, the monolith fails at 150 MPa, the CMC peaks at 400 MPa, and the area under its curve, the work of fracture, is about 49 times larger. Pull-out length scales as 1/τ: here up to 0.175 mm at τ = 20 MPa.

Which CMCs are in use, and what limits them?

The main families are carbon fibre in carbon (C/C), carbon fibre in SiC (C/SiC), SiC fibre in SiC (SiC/SiC) and oxide fibre in an oxide matrix (oxide/oxide). Carbon fibres and carbon interphases burn in hot air, so C/SiC and SiC/SiC parts carry coatings, and designers often keep working stresses below the matrix cracking stress, because cracks let oxygen reach the fibres. Oxide/oxide CMCs need no protection but lose strength at lower temperatures. In oxide CMCs a porous matrix itself provides the weak bond that a coating gives in the others.

Predict, then check

SiC fibres get a coating that bonds them strongly to the SiC matrix, raising Gi/Gf from 0.1 to 0.6. What happens to the composite?

Worked examples

Work of fracture of a CMC coupon · Illustrative model: 25 mm gauge, matrix cracking at 150 MPa, Vf 0.35, Ef 200 GPa, matrix 300 GPa, fibre bundle strength 1,000 MPa, fibre radius 7 µm and strength 1,000 MPa, interface sliding stress 25 MPa, weak interface.
  1. Composite modulus = 0.35 × 200 + 0.65 × 300 = 265 GPa; matrix cracks at δ = 150/265000 × 25 = 0.01415 mm
  2. Bridging: peak σu = 0.35 × 1,000 = 350 MPa, reached at δ = 0.01415 + (350 − 150)/(0.35 × 200,000) × 25 = 0.0856 mm
  3. Pull-out length u_po = σf r/(2τ) = 1,000 × 0.007/(2 × 25) = 0.14 mm; tail σu(1 − u/u_po)² has area σu u_po/3
  4. Areas: elastic 1.0613 + bridging 17.857 + pull-out 16.333 = 35.252 MPa·mm (kJ/m² of cross-section)
  5. Monolith (300 GPa): ½ × 150 × 0.0125 = 0.9375 MPa·mm

Answer: Work of fracture ≈ 35.3 kJ/m², about 38 times the monolith; pull-out supplies 46 % of it

Will the crack turn at the fibre? · SiC fibre fracture energy Gf = 20 J/m² (illustrative). Interface options: a pyrolytic carbon interphase, Gi = 2 J/m²; a strong oxide bond, Gi = 8 J/m². Similar fibre and matrix stiffness.
  1. Kinked-crack factors at 90°: kI = (3 cos 45° + cos 135°)/4 = 0.3536, kII = (sin 45° + sin 135°)/4 = 0.3536
  2. Energy released by turning ÷ by going straight = kI² + kII² = 0.25: the crack turns only if Gi/Gf is below this
  3. Carbon interphase: Gi/Gf = 2/20 = 0.1 < 0.25: deflects, the fibre survives
  4. Oxide bond: Gi/Gf = 8/20 = 0.4 > 0.25: the crack cuts the fibre
  5. Largest interface toughness that still deflects: 0.25 × 20 = 5 J/m²

Answer: Use the carbon (or BN) interphase; any Gi above about 5 J/m² makes the CMC brittle

Too few fibres to bridge · Same illustrative model with only Vf = 0.12 and τ = 10 MPa (weak interface).
  1. Fibres can carry the load after matrix cracking only if Vf × 1,000 > 150 MPa, so Vf must exceed 0.15
  2. At Vf = 0.12 they hold only 120 MPa: the stress drops from 150 to 120 MPa when the matrix cracks
  3. The fibres then pull out over u_po = 1,000 × 0.007/(2 × 10) = 0.35 mm, adding 120 × 0.35/3 = 14 MPa·mm
  4. Total work = 14.98 MPa·mm, 16 times the monolith, but the peak stays at 150 MPa

Answer: Not graceful: a load drop at cracking, then pull-out; raise Vf above 0.15 for rising, bridged behaviour

Chapter 12

Making CMCs: sintering, hot pressing, reaction bonding, infiltration, CVI, PIP, sol-gel and the Lanxide process

Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU not in syllabusMU MEDLO8051 Module 1KTU PEMET413 Module 4

Why are ceramic composites hard to make by pressing and sintering?

A plain ceramic is made by pressing powder and sintering it, letting atoms move until the pores close and the part shrinks. Fibres get in the way: they do not shrink, so the matrix around them cracks or stays porous, and the high sintering temperature can damage the fibres. Cold pressing and sintering suits particle or whisker reinforcement. For fibres, hot pressing helps: tows are drawn through a ceramic or glass slurry, stacked and pressed while hot, so pressure does the work that temperature alone cannot. Gentler routes infiltrate a fibre preform with a liquid or gas that becomes the matrix.

How does polymer infiltration and pyrolysis build up a matrix?

The fibre preform is soaked in a preceramic polymer, such as a polycarbosilane, which is cured and then pyrolysed to ceramic. Gas leaves and the material shrinks, so the ceramic fills only part of the pore space it soaked into. A model: each cycle fills a fraction yv of the open pores, so porosity falls geometrically. With an illustrative yv of 0.25 a preform at 55 % porosity needs 6 cycles to get below 10 %. In practice PIP needs five to eight cycles and leaves about 15 % porosity, partly because some pores close off and cannot be reached.

Densifying a ceramic composite: porosity after each polymer infiltration and pyrolysis cycle, and chemical vapour infiltration: interactive loads as you scroll

Why do the outer pores close first in chemical vapour infiltration?

In CVI a precursor gas flows round the hot preform, above 1000 °C, and deposits SiC on every fibre surface it reaches. The gas is used up as it diffuses inwards, so deposition is fastest near the faces. Those pores narrow first and finally seal, trapping porosity deeper inside: CVI parts typically keep 10-15 %. In the model, a slab with deposition-to-diffusion ratio (Thiele modulus) φ = 2 and 55 % starting porosity seals with 17 % average porosity. Slower, cooler, lower-pressure runs make φ smaller and the fill more even, at the cost of very long cycles.

What are reaction bonding, sol-gel and the Lanxide process?

Reaction bonding grows the matrix by a chemical reaction inside the part. In liquid silicon infiltration, molten silicon above 1414 °C wicks into a porous carbon preform and reacts, Si + C → SiC; the SiC takes up 2.29 times the volume of the carbon it replaces, filling pores to about 3 % porosity. Sol-gel soaks the preform in a colloidal solution that gels, dries and is fired to an oxide matrix at modest temperatures. The Lanxide (directed metal oxidation) process lets a molten aluminium alloy oxidise in air and grow an alumina matrix outward through a filler preform, leaving some metal behind.

Predict, then check

Each PIP cycle fills 30 % of the remaining open pores of a preform that starts at 50 % porosity. How many cycles until porosity is below 10 %?

Worked examples

Neat polymer or a 50 % solution? · A SiC fibre preform at 50 % porosity is densified by PIP. Polymer: ceramic yield 80 % by mass, density 1.1 g/cm³; the ceramic it leaves: 2.5 g/cm³ (illustrative). Compare soaking with neat polymer and with a 50 % solution.
  1. Neat: 1 cm³ of polymer (1.1 g) leaves 0.8 × 1.1 = 0.88 g of ceramic, 0.88/2.5 = 0.352 cm³: yv = 0.352
  2. Cycles to below 10 %: k > ln(0.1/0.5)/ln(1 − 0.352) = 3.71, so 4 cycles (porosity 8.8 %)
  3. 50 % solution: half the soaked volume is solvent, yv = 0.176; k > 8.31, so 9 cycles (porosity 8.8 %)
  4. Each cycle means a soak, a cure and a long pyrolysis, so a high-yield, solvent-free precursor saves whole cycles

Answer: 4 cycles with neat polymer against 9 with a 50 % solution

Reaction-bonded SiC: how much carbon? · Liquid silicon infiltrates a carbon preform that is 40 % carbon and 60 % open pores by volume. Si 28.085 g/mol, 2.329 g/cm³; C 12.011 g/mol, 2.2 g/cm³; SiC 40.096 g/mol, 3.21 g/cm³.
  1. Molar volumes: Si 12.06, C 5.46, SiC 12.49 cm³/mol
  2. Each cm³ of carbon becomes 12.49/5.46 = 2.288 cm³ of SiC, although Si + C → SiC shrinks the solids by 28.7 %
  3. 0.4 cm³ of carbon → 0.915 cm³ of SiC per cm³ of part; the remaining 0.085 cm³ fills with free silicon
  4. Silicon taken up by the reaction: 0.4/5.46 mol × 12.06 = 0.884 cm³ per cm³ of part, plus the 0.085 cm³ left as free Si
  5. Above 1/2.288 = 43.7 % carbon the new SiC would fill the pores before all the carbon reacts, choking the infiltration

Answer: About 92 % SiC and 8 % free silicon; keep carbon below about 44 vol%

Fast or slow CVI · A 50 % porous preform plate is densified by CVI; model profile c = cosh(φ(1 − x/L))/cosh φ, pores closing as r/r0 = 1 − τc. Compare φ = 1 (slow, low temperature) and φ = 3 (fast).
  1. Porosity left at seal (τ = 1) is p0(1 − c)²; its average is p0(1 − 2⟨c⟩ + ⟨c²⟩) with ⟨c⟩ = tanh φ/φ and ⟨c²⟩ = (sinh 2φ/(4φ) + ½)/cosh² φ
  2. φ = 1: ⟨c⟩ = 0.7616, ⟨c²⟩ = 0.5908, average porosity = 0.5 × 0.0676 = 3.4 %; centre 6.2 %
  3. φ = 3: average 25.4 %, centre 40.6 %
  4. A Simpson's-rule average of p0(1 − c)² across the plate gives the same values

Answer: Slow CVI seals at about 3 % porosity, fast CVI at 25 %: the fast run must be machined open and re-infiltrated

Chapter 13

Micromechanics: rule of mixtures, Halpin-Tsai and the strength of a unidirectional lamina

Which syllabus covers thisAU CME382 Unit IVTU not in syllabusSPPU 302052-A Units 3, 4MU MEDLO8051 Module 4KTU not in syllabus

Why is E1 a simple average of fibre and matrix, but E2 is not?

Along the fibres both phases stretch together (equal strain), so their stiffnesses add in proportion to volume: E1 = Ef Vf + Em Vm. For T300 carbon in 914C epoxy at Vf = 0.6 this gives 139.6 GPa, close to the measured lamina value of 138 GPa. Across the fibres the load passes through fibre and matrix in turn (equal stress), so compliances add: 1/E2 = Vf/Ef + Vm/Em. The soft epoxy dominates and the estimate is only 7.14 GPa against a measured 11 GPa. The basic rule of mixtures is also in the Engineering Materials and Metallurgy book.

What does the Halpin-Tsai equation add to the inverse rule of mixtures?

The inverse rule treats the lamina as slabs in series, which is the softest arrangement possible. Real round fibres let some load bypass the matrix. Halpin-Tsai interpolates between the two bounds with one factor ξ: ξ near 0 gives the inverse rule, a very large ξ gives the plain rule of mixtures. ξ = 2 is the usual choice for E2 and ξ = 1 for G12. For T300/914C at Vf = 0.6, E2 rises from 7.14 to 8.83 GPa. Matching the measured 17.7 GPa of E-glass/LY556 needs ξ ≈ 3.2, so ξ is really a fitted number; for T300/914C even the upper bound, 10.6 GPa, misses the measured 11 GPa.

Micromechanics: transverse and shear stiffness by the inverse rule and Halpin-Tsai, and longitudinal strength with the critical fibre volume: interactive loads as you scroll

Why must a carbon fibre's transverse modulus be used for E2?

A carbon fibre is itself anisotropic: its graphite layers line up along the axis, giving 230 GPa along it but only about 15 GPa across it (WWFE data for T300). Glass is isotropic, 80 GPa both ways. Putting the axial 230 GPa into the inverse rule for T300/914C at Vf = 0.6 gives E2 = 9.75 GPa instead of 7.14 GPa. The change is modest because the matrix term dominates, and it moves the estimate towards the measured 11 GPa for the wrong reason: the real lamina is made of a fibre that is soft across its axis.

How is the longitudinal strength estimated, and what are the minimum and critical fibre fractions?

With both phases elastic and strained equally, the weaker-strain phase breaks first. If the fibres break first (εfu below εmu), the composite fails at σ1 = σfu Vf + σ′m Vm, where σ′m = Em εfu is the matrix stress at that strain. At very low Vf the matrix alone, σmu Vm, can carry more, so fibres only add strength above Vcrit. For T300 (3,530 MPa) in 914C with an illustrative 75 MPa matrix strength, σ′m = 61.4 MPa and Vcrit = 0.39 %: tiny for a brittle polymer. The estimate at Vf = 0.6, 2,143 MPa, is well above the measured 1,500 MPa because fibres fail at their weakest flaws and are never perfectly aligned.

Predict, then check

Carbon/epoxy at Vf = 0.6 (fibre 230 GPa along, 15 GPa across; epoxy 4 GPa). If you wrongly used 230 GPa instead of 15 GPa in the inverse rule for E2, the estimate would…

Worked examples

All four elastic constants of AS4/3501-6 · AS4 fibre: E1f = 225 GPa, E2f = 15 GPa, G12f = 15 GPa, ν12f = 0.2; 3501-6 epoxy: Em = 4.2 GPa, Gm = 1.567 GPa, νm = 0.34 (WWFE data); Vf = 0.55
  1. E1 = 225 × 0.55 + 4.2 × 0.45 = 125.64 GPa
  2. ν12 = 0.2 × 0.55 + 0.34 × 0.45 = 0.263
  3. E2, inverse rule: 1/E2 = 0.55/15 + 0.45/4.2, so E2 = 6.95 GPa
  4. E2, Halpin-Tsai ξ = 2: η = (15/4.2 − 1)/(15/4.2 + 2) = 0.4615; E2 = 4.2 × (1 + 2 × 0.4615 × 0.55)/(1 − 0.4615 × 0.55) = 8.49 GPa
  5. G12, Halpin-Tsai ξ = 1: η = (15/1.567 − 1)/(15/1.567 + 1) = 0.8108; G12 = 4.09 GPa (inverse rule 3.09 GPa)

Answer: E1 ≈ 125.6 GPa, ν12 ≈ 0.26, E2 ≈ 8.5 GPa, G12 ≈ 4.09 GPa (Halpin-Tsai)

Fibre fraction for a target E1, then the transverse properties · E-glass fibre 80 GPa (isotropic, G = 33.33 GPa) in LY556 epoxy (3.35 GPa, G = 1.24 GPa); a bus-panel stiffener in a Hosur shop needs E1 = 40 GPa (illustrative)
  1. 40 = 80 Vf + 3.35 (1 − Vf), so Vf = (40 − 3.35)/(80 − 3.35) = 0.4781
  2. E2, inverse rule: 1/E2 = 0.478/80 + 0.522/3.35, so E2 = 6.18 GPa
  3. E2, Halpin-Tsai ξ = 2: 10.71 GPa
  4. G12, Halpin-Tsai ξ = 1: 3.22 GPa

Answer: Vf ≈ 0.48; E2 ≈ 10.7 GPa and G12 ≈ 3.22 GPa by Halpin-Tsai

Minimum and critical fibre fraction for a tough matrix · T300 fibre: σfu = 3,530 MPa, Ef = 230 GPa; an illustrative toughened matrix: σmu = 120 MPa, Em = 3.0 GPa, failure strain 4 %
  1. Fibre failure strain εfu = 3530/230000 = 1.535 %, below the matrix's 4 %, so the fibres break first
  2. Matrix stress when the fibres break: σ′m = 3000 × 0.01535 = 46.04 MPa
  3. Vmin = (σmu − σ′m)/(σfu + σmu − σ′m) = (120 − 46.04)/(3530 + 120 − 46.04) = 0.0205
  4. Vcrit = (σmu − σ′m)/(σfu − σ′m) = 73.96/3484 = 0.0212
  5. At Vf = 0.5: σ1 = 3530 × 0.5 + 46.04 × 0.5 = 1788 MPa

Answer: Vmin ≈ 2.05 %, Vcrit ≈ 2.12 %, σ1 ≈ 1,788 MPa at Vf = 0.5

Chapter 14

Short-fibre composites: shear lag, critical fibre length and fibre orientation

Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302052-A Unit 4MU not in syllabusKTU not in syllabus

How does load get into a short fibre?

The matrix grips the fibre by shear at the interface. At a fibre end the fibre stress is zero; it builds up over a transfer length as shear is passed in, then levels off near the strain the matrix imposes. Cox's elastic shear-lag model gives a cosh-shaped stress profile and shear concentrated at the ends. The fibre's average stress, as a fraction of the long-fibre value, is the length efficiency ηl. For E-glass in LY556 epoxy at Vf = 0.2 and l/d = 20, ηl = 0.765, so the modulus is about 14.9 GPa instead of 18.68 GPa for continuous fibres.

Short fibres: stress building up along a fibre by shear lag, the critical length and the efficiency of random orientation: interactive loads as you scroll

What is the critical fibre length?

If the interface can carry at most a shear stress τ (it slips or the matrix yields), the fibre stress rises linearly from each end at 4τ/d. It reaches the fibre strength σfu only if each half is at least σfu d/(4τ) long, so the critical length is lc = σfu d/(2τ) (Kelly-Tyson). For E-glass (3,445 MPa) with an illustrative τ = 40 MPa and 14 µm diameter, lc/d ≈ 43 and lc ≈ 0.6 mm. Shorter fibres pull out before breaking; a fibre exactly lc long delivers only half of its strength on average.

How much stiffness is lost when short fibres point in random directions?

A fibre at angle θ to the load adds stiffness in proportion to cos⁴θ: one cos² because only that share of the strain stretches it, one cos² because only that share of its force points along the load. Averaging cos⁴θ gives Krenchel's orientation efficiency: 1 for aligned fibres, 3/8 for fibres random in a plane, and 1/5 for fibres random in 3-D. In E ≈ ηo ηl Ef Vf + Em Vm, the glass/epoxy above at l/d = 100 and random in-plane drops to about 8.4 GPa, so orientation usually costs more than length.

Why use short fibres at all?

Short fibres let a composite flow. Chopped glass in a polyester sheet or bulk moulding compound fills a compression mould, and glass-filled nylon or polypropylene pellets run in an ordinary injection-moulding machine, so a part with ribs, bosses and clips comes out in one shot at high volume. The price is lower stiffness and strength than continuous fibres, because fibres break during compounding and moulding and the flow sets their orientation. The Manufacturing Processes book covers the injection-moulding machine itself.

Predict, then check

Short fibres exactly as long as the critical length lc are loaded until they break. What fraction of the fibre strength do they deliver on average along their length?

Worked examples

Critical length of a chopped carbon fibre · T300 carbon fibre: σfu = 3,530 MPa; an illustrative diameter of 7 µm and interfacial shear strength τ = 50 MPa; fibres chopped to 3 mm for a drone-arm moulding compound
  1. lc = σfu d/(2τ) = 3530 × 0.007/(2 × 50) = 0.2471 mm
  2. l/lc = 3/0.2471 = 12.14
  3. Strength efficiency (l ≥ lc): 1 − lc/(2l) = 1 − 1/(2 × 12.14) = 0.959

Answer: lc ≈ 0.25 mm; 3 mm fibres deliver about 96 % of the fibre strength

Modulus of a short glass-fibre moulding by shear lag and Krenchel · E-glass fibre Ef = 80 GPa in LY556 epoxy (Em = 3.35 GPa, Gm = 1.24 GPa), Vf = 0.3, l/d = 50; square packing, R = half the fibre spacing
  1. ln(R/r) = ½ ln(π/(4 × 0.3)) = 0.4812
  2. βr = √(2Gm/(Ef ln(R/r))) = √(2 × 1.24/(80 × 0.4812)) = 0.2538; βl/2 = βr × l/d = 12.691
  3. ηl = 1 − tanh(12.691)/12.691 = 0.9212
  4. Aligned: E = 0.9212 × 80 × 0.3 + 3.35 × 0.7 = 24.45 GPa
  5. Random in-plane (ηo = 3/8): 10.64 GPa; random 3-D (ηo = 1/5): 6.77 GPa

Answer: E ≈ 24.5 GPa aligned, 10.6 GPa random in-plane, 6.8 GPa random 3-D

Strength of aligned short glass fibres, longer and shorter than lc · E-glass σfu = 3,445 MPa, lc = 0.6 mm (from τ = 40 MPa, d = 14 µm, illustrative), Vf = 0.25, matrix stress at failure σ′m = 40 MPa (illustrative)
  1. l = 1.2 mm (l ≥ lc): σc = σfu Vf (1 − lc/(2l)) + σ′m Vm = 3445 × 0.25 × (1 − 0.6/2.4) + 40 × 0.75 = 675.9 MPa
  2. l = 0.3 mm (l below lc): σc = σfu Vf l/(2lc) + σ′m Vm = 3445 × 0.25 × 0.3/1.2 + 40 × 0.75 = 245.3 MPa
  3. Continuous fibres for comparison: 3445 × 0.25 + 40 × 0.75 = 891.2 MPa

Answer: ≈ 676 MPa with 1.2 mm fibres and 245 MPa with 0.3 mm fibres (76 % and 28 % of continuous)

Chapter 15

Hooke's law for a lamina: orthotropic stiffness [Q] and compliance [S]

Which syllabus covers thisAU CME382 Unit IVTU not in syllabusSPPU not in syllabusMU MEDLO8051 Module 2KTU not in syllabus

Why does a unidirectional lamina need four elastic constants?

A lamina is orthotropic: it has three planes of symmetry, one along the fibres (axis 1), one across them (axis 2) and the ply plane. In a thin ply loaded in its own plane (plane stress), four numbers describe it: E1, E2, ν12 and G12. A fifth, ν21, is not independent: reciprocity requires ν21/E2 = ν12/E1. For carbon/epoxy T300/914C (E1 = 138 GPa, E2 = 11 GPa, ν12 = 0.28), ν21 = 0.28 × 11/138 = 0.0223: pulling along the fibres narrows the ply a lot, pulling across them barely shortens it.

What are the compliance matrix [S] and the reduced stiffness matrix [Q]?

[S] turns stresses into strains: ε1 = σ1/E1 − ν12σ2/E1, ε2 = −ν12σ1/E1 + σ2/E2, γ12 = τ12/G12. [Q] is its inverse and turns strains into stresses. For T300/914C, Q11 = 138.87 GPa, slightly above E1 because the ply is held against the Poisson contraction. With σ1 = 400, σ2 = 20 and τ12 = 30 MPa the strains are 2,858, 1,007 and 5,455 µε: the small transverse stress produces a strain a third the size of the fibre strain.

Hooke's law for a lamina: the stiffness and compliance matrices, and how an element strains along and across the fibres: interactive loads as you scroll

Why is there no shear-extension coupling on the material axes?

On the 1-2 axes the fibres are a mirror symmetry of the ply: flipping axis 2 does not change the material, so a normal stress cannot make the element shear one way rather than the other. That is why S16, S26, Q16 and Q26 are zero, and the element in the interactive only shears when you apply τ12. Load the same ply on axes turned away from the fibres and the symmetry is lost: the terms appear and a pure pull makes it shear. That is the angle lamina of the next chapter.

What happens to [Q] when the lamina becomes isotropic?

Set E1 = E2 = E and ν12 = ν, and G is no longer free: it must be E/(2(1 + ν)). Then Q66 = (Q11 − Q12)/2, the same condition the A matrix of a quasi-isotropic laminate meets later. For LY556 epoxy (E = 3.35 GPa, ν = 0.35), Q11 = 3.818 GPa, Q12 = 1.336 GPa and Q66 = 1.241 GPa. An orthotropic ply has four independent constants; an isotropic one has two.

Can any four numbers be the constants of a lamina?

No. Stretching or shearing a material must store positive energy, so [S] and [Q] must be positive definite. That needs E1, E2 and G12 positive and ν12² below E1/E2. For T300/914C the limit is ν12 below √(138/11) = 3.54, so 0.28 is far inside it; for an isotropic material the same rule gives ν below 1, and the 3-D rule tightens it to ν below 0.5. A test value outside these limits means a measurement error, not a strange material.

Predict, then check

Carbon/epoxy (E1 = 138 GPa, E2 = 11 GPa, ν12 = 0.28) is pulled across the fibres with σ2 = 20 MPa. How much does it strain along the fibres?

Worked examples

[S] and [Q] of E-glass/epoxy · E-glass/LY556: E1 = 53.48 GPa, E2 = 17.7 GPa, ν12 = 0.278, G12 = 5.83 GPa (WWFE data)
  1. S11 = 1/E1 = 18.699 /TPa; S12 = −ν12/E1 = −5.198 /TPa; S22 = 1/E2 = 56.5 /TPa; S66 = 1/G12 = 171.5 /TPa
  2. ν21 = 0.278 × 17.7/53.48 = 0.092; 1 − ν12ν21 = 0.9744
  3. Q11 = 53.48/0.9744 = 54.88 GPa; Q22 = 17.7/0.9744 = 18.16 GPa
  4. Q12 = ν12E2/(1 − ν12ν21) = 5.05 GPa; Q66 = G12 = 5.83 GPa
  5. Check: inverting [S] numerically gives the same [Q] to rounding

Answer: Q11 ≈ 54.9, Q12 ≈ 5.05, Q22 ≈ 18.2, Q66 = 5.83 GPa

Strains in a Kevlar/epoxy ply · Kevlar/epoxy: E1 = 80 GPa, E2 = 5.5 GPa, ν12 = 0.31, G12 = 2.1 GPa; σ1 = 600 MPa, σ2 = −40 MPa, τ12 = 15 MPa (illustrative)
  1. ε1 = 600/80000 − 0.31 × (−40)/80000 = 7,655 µε
  2. ε2 = −0.31 × 600/80000 + (−40)/5500 = −9,598 µε
  3. γ12 = 15/2100 = 7,143 µε
  4. The 40 MPa transverse compression strains the ply more than the 600 MPa pull along the fibres does

Answer: ε1 ≈ 7,655 µε, ε2 ≈ −9,598 µε, γ12 ≈ 7,143 µε

Stresses from strain-gauge readings on a HM carbon ply · HM carbon/epoxy: E1 = 230 GPa, E2 = 6.6 GPa, ν12 = 0.25, G12 = 4.8 GPa; a rosette on a spar cap reads ε1 = 1,500 µε, ε2 = −300 µε, γ12 = 2,000 µε (illustrative)
  1. ν21 = 0.25 × 6.6/230 = 0.00717; 1 − ν12ν21 = 0.99821
  2. Q11 = 230.4 GPa, Q12 = 1.653 GPa, Q22 = 6.612 GPa, Q66 = 4.8 GPa
  3. σ1 = Q11 ε1 + Q12 ε2 = 345.1 MPa
  4. σ2 = Q12 ε1 + Q22 ε2 = 0.5 MPa
  5. τ12 = Q66 γ12 = 9.6 MPa

Answer: σ1 ≈ 345 MPa, σ2 ≈ 0.5 MPa, τ12 ≈ 9.6 MPa

Chapter 16

The angle lamina: transformation, [Q̄] and off-axis engineering constants

Which syllabus covers thisAU CME382 Unit IVTU not in syllabusSPPU not in syllabusMU MEDLO8051 Module 2KTU not in syllabus

How are stresses moved from the x-y axes to the fibre axes?

A ply in a laminate rarely has its fibres along the load. With the fibre at θ counter-clockwise from x, the stress transformation (the same algebra as Mohr's circle) gives σ1 = c²σx + s²σy + 2csτxy, σ2 = s²σx + c²σy − 2csτxy and τ12 = −csσx + csσy + (c² − s²)τxy, with c = cos θ and s = sin θ. A pull of σx = 100 MPa on a 30° ply becomes σ1 = 75, σ2 = 25 and τ12 = −43.3 MPa. Strains transform the same way if half the engineering shear strain is used.

What is the transformed stiffness [Q̄] of a ply?

[Q̄] relates x-y stresses to x-y strains for a ply at θ. It is [Q] rotated: transform the strains to 1-2, apply [Q], and transform the stresses back. Unlike [Q] it is fully populated: Q̄16 and Q̄26 are non-zero for any angle other than 0° and 90°. For T300/914C at 30°, Q̄11 = 84.1 GPa and Q̄16 = 40.8 GPa; at −30° Q̄16 is exactly −40.8 GPa. That sign flip is why a +θ ply paired with a −θ ply cancels the coupling in a balanced laminate.

Why does an angle ply shear when it is only pulled?

The ply is stiff along its fibres and soft across them, so under a pull along x it stretches most in the soft direction, which is not along x. A square drawn on it skews into a parallelogram. The ratio ηxy,x = γxy/εx measures this shear-extension coupling. For T300/914C at 30° it is −1.24: for every unit of stretch the element shears 1.24 units. The coupling peaks at about 11.1°, where |ηxy,x| = 2.25, and it is zero at 0° and 90°. A test coupon cut slightly off-axis twists in its grips for this reason.

The angle lamina: shear coupling under pure tension, and the off-axis modulus, shear modulus and Poisson's ratio against angle: interactive loads as you scroll

How fast do the stiffnesses change with fibre angle?

Very fast near 0°. For T300/914C, Ex is 138 GPa along the fibres but 82.7 GPa at 10°, 56.1 GPa at 15° and 23.2 GPa at 30°, because the soft shear term takes over as soon as the fibres tilt. Gxy behaves the other way: it is lowest on-axis (5.5 GPa) and highest at 45° (9.78 GPa), where the fibres carry the shear as tension and compression. νxy peaks at 0.41 near 22°. A few degrees of fibre misalignment from layup cost a large share of the stiffness.

Predict, then check

The fibres of a carbon/epoxy ply (E1 = 138 GPa, E2 = 11 GPa, G12 = 5.5 GPa, ν12 = 0.28) are 15° off the load. Its modulus along the load is closest to…

Worked examples

Engineering constants of a 45° glass ply · E-glass/LY556: E1 = 53.48 GPa, E2 = 17.7 GPa, ν12 = 0.278, G12 = 5.83 GPa; fibres at 45° to x
  1. At 45°: c² = s² = 0.5, so c⁴ = s⁴ = s²c² = 0.25
  2. 1/Ex = 0.25/53.48 + (1/5.83 − 2 × 0.278/53.48) × 0.25 + 0.25/17.7 = 0.05908 /GPa, so Ex = 16.93 GPa
  3. Gxy = 11.68 GPa, double the on-axis 5.83 GPa
  4. νxy = 0.452; ηxy,x = −0.32 (not zero: E1 ≠ E2)

Answer: Ex ≈ 16.9 GPa, Gxy ≈ 11.7 GPa, νxy ≈ 0.45

Strains of a 30° carbon ply under a pure pull · T300/914C (E1 = 138, E2 = 11, G12 = 5.5 GPa, ν12 = 0.28), fibres at 30°, σx = 100 MPa, σy = τxy = 0
  1. Local stresses: σ1 = 0.75 × 100 = 75 MPa, σ2 = 0.25 × 100 = 25 MPa, τ12 = −0.433 × 100 = −43.3 MPa
  2. Local strains: ε1 = 492.8 µε, ε2 = 2,121 µε, γ12 = −7,873 µε
  3. Back to x-y (half the shear strain transforms): εx = 4,309 µε, εy = −1,695 µε, γxy = −5,346 µε
  4. Check: Ex = 100/εx = 23.21 GPa and γxy/εx = −1.241, as the closed forms give

Answer: εx ≈ 4,309 µε, εy ≈ −1,695 µε, γxy ≈ −5,346 µε: it shears under a pure pull

[Q̄] of a ±60° Kevlar pair · Kevlar/epoxy: E1 = 80 GPa, E2 = 5.5 GPa, ν12 = 0.31, G12 = 2.1 GPa; plies at +60° and −60°
  1. [Q]: Q11 = 80.53, Q12 = 1.716, Q22 = 5.537, Q66 = 2.1 GPa
  2. +60°: Q̄11 = 10.37, Q̄22 = 47.86, Q̄12 = 15.64, Q̄66 = 16.02, Q̄16 = 8.2, Q̄26 = 24.27 GPa
  3. −60°: the same except Q̄16 = −8.2 and Q̄26 = −24.27 GPa
  4. Averaging the pair cancels Q̄16 and Q̄26; a single +60° ply has Ex = 5.24 GPa and ηxy,x = −0.073

Answer: Q̄22 ≈ 47.9 GPa (60° is close to the y axis); Q̄16 = ±8.2 GPa cancels in the ±60° pair

Chapter 17

Laminate codes: symmetric, balanced, cross-ply, angle-ply and quasi-isotropic laminates

Which syllabus covers thisAU CME382 Unit IIVTU not in syllabusSPPU 302052-A Unit 2MU MEDLO8051 Module 4KTU not in syllabus

How do you read a stacking code such as [0/±45/90]s?

Plies are listed from the top surface down, angles in degrees from the x axis. ±45 means a +45 ply then a −45 ply. A subscript repeats one ply (0₂ is two 0° plies), a number after the bracket repeats the whole group ([0/90]2 is 0/90/0/90), and s mirrors everything about the mid-plane. So [0/±45/90]s is 0/45/−45/90/90/−45/45/0: 8 plies, 1 mm thick with a typical 0.125 mm ply. For an odd symmetric laminate a bar over the last angle marks the single middle ply. Build codes in the interactive; each one is parsed back to prove it is unambiguous.

Build a laminate ply by ply: the stacking code, symmetric, balanced, cross-ply, angle-ply and quasi-isotropic checks: interactive loads as you scroll

What do symmetric and balanced buy you?

Symmetric means every ply has a twin of the same angle at the same distance on the other side of the mid-plane. Then B = 0: pulling does not bend and cooling after cure does not warp. Balanced means every +θ ply has a −θ ply somewhere, so A16 = A26 = 0: pulling does not shear. They are independent. In carbon/epoxy the two-ply [0/45] is neither: B11 = −737 N and A16 = 3.99 kN/mm. [±45] is balanced but not symmetric, so B16 = −499 N and it twists when pulled.

What are cross-ply, angle-ply and antisymmetric laminates?

A cross-ply has only 0° and 90° plies; an angle-ply has only +θ and −θ plies of one angle. Antisymmetric means each ply is mirrored by its opposite: −θ for +θ, or 90° for 0°, as in [0/90]2 and [±45]2. Antisymmetric cross-plies keep only B11 = −B22; antisymmetric angle-plies keep only B16 and B26. The coupling fades as plies are added: at the same average stress, the curl of carbon [0/90]4 is 3 % of that of the two-ply [0/90], because B grows with n but D grows with n³.

What makes a laminate quasi-isotropic, and is it really isotropic?

Use n ≥ 3 fibre directions spaced 180°/n apart with the same number of plies in each: [0/±60]s (n = 3) or [0/±45/90]s (n = 4). Then A11 = A22, A16 = A26 = 0 and A66 = (A11 − A12)/2, exactly the form of an isotropic plate, so the in-plane stiffness is the same in every direction. Only in-plane: for carbon [0/±45/90]s, D11 = 8,212 N·mm but D22 = 2,222 N·mm, because the 0° plies sit outside. The interactive checks the three conditions numerically on A, not by looking at the angles.

Predict, then check

A carbon/epoxy laminate is laid up 0/45/−45/90 from the top and NOT mirrored. Which statement is true?

Worked examples

Expanding a stacking code · [0₂/±30/90]s with a typical 0.125 mm ply (illustrative)
  1. Write the half before s: 0, 0, +30, −30, 90
  2. Mirror it: 0/0/30/−30/90/90/−30/30/0/0, which is 10 plies
  3. Thickness h = 10 × 0.125 = 1.25 mm, so ply 1 runs from z = −0.625 mm to −0.5 mm and the two 90° plies meet at z = 0
  4. Count: four 0°, two +30°, two −30°, two 90°; every +30 has a −30, so it is balanced (A16 = A26 = 0)
  5. Every ply has a twin at −z, so it is symmetric (B = 0). It is not quasi-isotropic: the directions are not 180°/n apart

Answer: 10 plies, 1.25 mm, symmetric and balanced

Checking [0/±60]s for quasi-isotropy · E-glass/epoxy LY556: E1 = 53.48 GPa, E2 = 17.7 GPa, ν12 = 0.278, G12 = 5.83 GPa; 0.125 mm plies
  1. Q11 = 54,884 MPa, Q12 = 5,050 MPa, Q22 = 18,165 MPa, Q66 = 5,830 MPa
  2. Q̄11 at ±60° = 19,914 MPa; with two plies of each angle, A11 = 0.25 × (54,884 + 2 × 19,914) = 23,678 N/mm
  3. A22 = 23,678 N/mm, A12 = 7,502.5 N/mm, A66 = 8,087.7 N/mm
  4. (A11 − A12)/2 = 8,087.7 N/mm = A66, and A16 = A26 = 0 (±60 pairs)
  5. A11/h = 31,571 MPa, the invariant U1 = (3Q11 + 3Q22 + 2Q12 + 4Q66)/8 of the ply

Answer: Yes in-plane (A11 = A22 = 23.68 kN/mm); but D11 = 1,565 and D22 = 848.1 N·mm differ

How fast does cross-ply coupling fade? · Carbon/epoxy [0/90], [0/90]2 and [0/90]4 (2, 4, 8 plies of 0.125 mm), each pulled to an average stress of 100 MPa
  1. [0/90]: B11 = (t²/2)(Q22 − Q11) = −998.4 N; Nx = 25 N/mm gives εx0 = 2,942 µε and κx = 30.09 1/m
  2. [0/90]2: B11 = −1,997 N (twice), but D is 8 times larger; Nx = 50 N/mm gives κx = 3.96 1/m
  3. [0/90]4: B11 = −3,994 N; Nx = 100 N/mm gives κx = 0.88 1/m
  4. Surface bending strain κx·h/2 against εx0: 1.279, 0.639, 0.32

Answer: κx falls from 30.1 to 4 to 0.88 1/m as the plies double; only a symmetric layup removes it

Chapter 18

Classical laminate theory: resultants, the [A], [B] and [D] matrices and coupling

Which syllabus covers thisAU CME382 Unit IIVTU not in syllabusSPPU not in syllabusMU not in syllabusKTU not in syllabus

What are force and moment resultants, and what does CLT assume?

Stresses change from ply to ply, so a laminate is loaded by their totals per unit width: Nx is the integral of σx through the thickness (N/mm) and Mx the integral of σx·z (N·mm/mm). Classical laminate theory assumes thin plies perfectly bonded and straight normals that stay normal, so the strain is linear in z: ε = ε0 + zκ, a mid-plane strain plus z times a curvature. A 1 mm carbon [0/±45/90]s with Nx = 100 N/mm carries an average 100 MPa and stretches 1,847 µε.

What do A, B and D mean physically?

N = A·ε0 + B·κ and M = B·ε0 + D·κ. A is in-plane stiffness: each ply's Q̄ times its thickness, so stacking order does not matter. D is bending stiffness: Q̄ times (z₁³ − z₀³)/3, so outer plies dominate. B couples the two and weights each ply by (z₁² − z₀²)/2, which is negative above the mid-plane and positive below, so mirrored twins cancel. Units: A in N/mm, B in N, D in N·mm. The 6 × 6 matrix is inverted once to get strains and curvatures from loads.

Why does an unsymmetric laminate curl when you pull it?

With B ≠ 0 a pull also produces curvature. In carbon/epoxy [0/90] (two 0.125 mm plies) B11 = −998 N and B22 = +998 N. In the interactive's default, Nx = 60 N/mm gives εx0 = 7,060 µε and κx = 72.2 1/m: the stiff 0° ply on top takes the load off-centre and the strip bows. Switch to [±45] and B16, B26 make it twist instead. The same coupling warps unsymmetric parts as they cool from the cure temperature.

The A, B and D matrices of a laminate, and an unsymmetric laminate that bends and twists when you pull it: interactive loads as you scroll

What do A16 and D16 terms do?

A16 and A26 couple stretching to in-plane shear; they vanish in balanced laminates. D16 and D26 couple bending to twisting, and they survive in a symmetric balanced laminate whenever a +θ and its −θ ply sit at different depths. In carbon [0/±45/90]s, D16 = D26 = 499 N·mm against D11 = 8,212 N·mm, so a pure Mx also twists the plate slightly. Interleaving +θ and −θ plies through the thickness, or using woven ±45 fabric, shrinks D16.

Predict, then check

A two-ply carbon/epoxy laminate +45/−45 (top to bottom) is pulled along x. What does it do besides stretch?

Worked examples

A and D of [0/90]s by hand · E-glass/epoxy LY556 [0/90]s, four 0.125 mm plies, h = 0.5 mm
  1. Q11 = 54,884, Q12 = 5,050, Q22 = 18,165, Q66 = 5,830 MPa; for a 90° ply Q11 and Q22 swap
  2. A11 = 0.25 × (Q11 + Q22) = 18,262 N/mm = A22; A12 = 0.5 × Q12 = 2,525 N/mm; A66 = 0.5 × Q66 = 2,915 N/mm
  3. B = 0: every ply has a twin at −z, and (z₁² − z₀²) changes sign
  4. D11 = (2/3)[Q11(0.25³ − 0.125³) + Q22 × 0.125³] = 523.9 N·mm
  5. D22 = (2/3)[Q22(0.25³ − 0.125³) + Q11 × 0.125³] = 237 N·mm

Answer: A11 = A22 = 18.26 kN/mm, B = 0, D11 = 523.9 N·mm is 2.21 × D22 (0° plies outside)

Pulling an unsymmetric [0/90] · Carbon/epoxy [0/90], 0° ply on top, two 0.125 mm plies, Nx = 20 N/mm (illustrative)
  1. A11 = A22 = 18,742 N/mm, A12 = 774.8 N/mm; B11 = −B22 = −998.4 N; D11 = D22 = 97.62 N·mm, D12 = 4.04 N·mm
  2. Shear terms are uncoupled, so four equations remain in εx0, εy0, κx, κy: Nx = A11εx0 + A12εy0 + B11κx, 0 = A12εx0 + A22εy0 − B11κy, 0 = B11εx0 + D11κx + D12κy, 0 = −B11εy0 + D12κx + D22κy
  3. Solving: εx0 = 2,353 µε, εy0 = −97 µε, κx = 24.07 1/m and κy = 0 (B12 = 0 and the D12 and B22 terms balance)
  4. Without coupling εx0 would be Nx/(A11 − A12²/A22) = 1,069 µε: the curl adds stretch at the mid-plane
  5. Radius of curvature 1/κx = 42 mm in linear theory

Answer: εx0 = 2,353 µε and κx = 24.1 1/m: it bends while it stretches

Bend-twist in a quasi-isotropic plate · Carbon/epoxy [0/±45/90]s, h = 1 mm, Mx = 2 N·mm/mm (illustrative)
  1. B = 0, so κ = D⁻¹M: D11 = 8,212, D12 = 1,289, D22 = 2,222, D16 = D26 = 499.2, D66 = 1,489 N·mm
  2. Inverting D: d11 = 134.535 × 10⁻⁶, d61 = −20.493 × 10⁻⁶ 1/(N·mm)
  3. κx = d11 × 2 = 0.2691 1/m; κxy = d61 × 2 = −0.041 1/m
  4. Ignoring D12 and D16 (κx = Mx/D11) gives 0.2435 1/m, an error of 10.5 %

Answer: κx = 0.269 1/m with a small twist κxy = −0.041 1/m from D16

Chapter 19

Strains and stresses ply by ply through a laminate

Which syllabus covers thisAU CME382 Unit IIVTU not in syllabusSPPU not in syllabusMU not in syllabusKTU not in syllabus

How does strain vary through the thickness of a laminate?

Linearly and continuously: ε(z) = ε0 + zκ, the same straight line through every ply, because the plies are bonded and the normals stay straight. Under in-plane loads alone a symmetric laminate has κ = 0, so every ply sees the same strain. Under a moment the strain is zero at the mid-plane and largest at the faces. Strain never jumps at an interface; if it did, the plies would slide over each other. Find ε0 and κ from the inverted ABD matrix first, then everything else follows ply by ply.

Why does stress jump at a ply interface?

Each ply turns the same strain into stress with its own Q̄: σ = Q̄(ε0 + zκ). At an interface the strain is equal on both sides but Q̄ changes, so σx jumps. In carbon [0/90]s pulled along x, a 0° ply carries 12.7 times the σx of a 90° ply at the same strain. In the interactive's default ([0/±45/90]s, Nx = 100 N/mm) the 0° plies carry σ1 = 255 MPa while the 90° plies carry σ2 = 18.7 MPa across their fibres. The stresses still add up exactly to N and M.

Through the thickness: strain linear in z, stress jumping from ply to ply, and the fibre and transverse stress in each ply: interactive loads as you scroll

Why transform ply stresses to the fibre axes?

Strength is known along and across the fibres (Xt, Yt, S), so failure checks need σ1, σ2 and τ12 in each ply's own axes, found by rotating σx, σy, τxy through θ. In the default above, the transverse stress in the 90° plies is the critical one: σ2 = 18.69 MPa against Yt = 27 MPa for T300/914C, a strength ratio of 1.44. That is why the first cracks in a cross-ply usually appear in the 90° plies, long before any fibre breaks. Chapter 21 turns these ratios into failure criteria.

Where are the highest stresses when a laminate is bent?

Under a moment the strain is largest at the faces, and the stress also depends on the ply's stiffness, so the peak is at the outer face of the stiffest outer ply, and there is a jump inside at each interface. In carbon [0/90]s with Mx = 1 N·mm/mm (Example 2), σx is −27.1 MPa at the top face, −13.6 MPa at the bottom of the top 0° ply, but only −1.05 MPa just below it in the 90° ply. Putting 0° plies outside is how bending stiffness is bought cheaply.

Predict, then check

A carbon/epoxy [0/90]s laminate is pulled along x. Compared with a 90° ply, how much σx does a 0° ply carry?

Worked examples

Ply stresses in a pulled cross-ply · Carbon/epoxy [0/90]s, four 0.125 mm plies, Nx = 50 N/mm (illustrative)
  1. A11 = A22 = 37,484 N/mm, A12 = 1,550 N/mm, B = 0
  2. εx0 = Nx·A22/(A11A22 − A12²) = 1,336.2 µε; εy0 = −Nx·A12/(A11A22 − A12²) = −55.24 µε
  3. 0° plies: σx = Q11εx + Q12εy = 185.38 MPa (= σ1); σy = Q12εx + Q22εy = 3.53 MPa (= σ2)
  4. 90° plies: σx = Q22εx + Q12εy = 14.62 MPa (= σ2); σy = Q12εx + Q11εy = −3.53 MPa (= σ1)
  5. Check: 0.25 × (185.38 + 14.62) = 50 N/mm = Nx, and the σy values cancel, so Ny = 0

Answer: σ1 = 185.4 MPa in the 0° plies, σ2 = 14.62 MPa across the 90° plies

Stress jump under bending · The same [0/90]s, Mx = 1 N·mm/mm (illustrative)
  1. D11 = 1,280, D12 = 32.3, D22 = 281.7 N·mm; κx = D22/(D11D22 − D12²) = 0.7834 1/m, κy = −0.0898 1/m
  2. Top face z = −0.25 mm: εx = −195.9 µε, σx = −27.13 MPa
  3. Interface z = −0.125 mm: εx = −97.9 µε in both plies
  4. σx = −13.56 MPa on the 0° side and −1.049 MPa on the 90° side: a jump of 12.52 MPa
  5. Check: the integral of σx·z through the thickness = 1 N·mm/mm = Mx

Answer: Peak σx = −27.1 MPa at the faces; at the interface σx drops from −13.6 to −1.05 MPa

Why ±45 plies carry shear · Carbon/epoxy [±45]s, h = 0.5 mm, Nxy = 20 N/mm (illustrative)
  1. A66 = 17,967 N/mm, so γxy = Nxy/A66 = 1,113 µε (A16 = 0, B = 0)
  2. Every ply carries τxy = Nxy/h = 40 MPa; with εx = εy = 0 the +45 ply also carries σx = σy = Q̄16·γxy = 35.56 MPa and the −45 ply the opposite, so they cancel in Nx and Ny
  3. +45 ply: σ1 = (σx + σy)/2 + τxy = 75.56 MPa, σ2 = (σx + σy)/2 − τxy = −4.44 MPa, τ12 = 0
  4. −45 ply: σ1 = −75.56 MPa, σ2 = 4.44 MPa: the shear becomes fibre tension in one ply and fibre compression in the other
  5. Shear stiffness Gxy = A66/h = 35.93 GPa, against 5.5 GPa for [0/90]s

Answer: σ1 = ±75.6 MPa along the fibres, τ12 = 0; [±45]s is 6.5 times stiffer in shear than [0/90]s

Chapter 20

Laminate engineering constants and lamina properties from laminate tests

Which syllabus covers thisAU CME382 Unit IIVTU not in syllabusSPPU not in syllabusMU MEDLO8051 Module 4KTU not in syllabus

How do you get Ex, Ey, νxy and Gxy of a laminate?

For a symmetric laminate (B = 0) invert A and divide by the thickness: Ex = 1/(h·a11), Ey = 1/(h·a22), Gxy = 1/(h·a66), νxy = −a12/a11, where a = A⁻¹. They describe the laminate as one homogeneous plate under in-plane loads. Carbon/epoxy [0/90]2s gives Ex = Ey = 74.84 GPa, close to the average of E1 and E2 (74.5 GPa), but Gxy = 5.5 GPa, no better than one ply, and νxy = 0.041. Quasi-isotropic [0/±45/90]s gives 54.14 GPa in every direction.

How does a laminate's modulus change with direction?

Load a laminate at an angle φ and its plies sit at θ − φ to the load, so Ex(φ) is a polar curve. A UD ply is a narrow figure of eight; a cross-ply has lobes at 0° and 90°; a quasi-isotropic layup is a circle. Angle-plies have a surprise: νxy of carbon [±θ]s peaks at 1.316 near θ = 26.7°, above the 0.5 an isotropic solid can reach, because the plies scissor. E-glass peaks at only 0.64. The interactive plots the polar curve and these curves.

Laminate moduli in every direction, cross-ply and angle-ply laminates, and backing out the shear modulus from a ±45 test: interactive loads as you scroll

Why is the bending modulus of a laminate different from its in-plane modulus?

In-plane moduli come from A, where every ply counts equally. The flexural modulus Exf = 12/(h³·d11), from D⁻¹, weights plies by z², so the outer plies dominate. Carbon [0/±45/90]s has Ex = 54.1 GPa in-plane but Exf = 89.2 GPa in bending, because its 0° plies are outside; Eyf is only 22.8 GPa. Reordering the plies changes the bending stiffness but never the in-plane stiffness, a simple lever for designing a stiff panel.

How are lamina properties measured with laminate tests?

G12 is measured by pulling a symmetric, balanced ±45 coupon (ISO 14129, the counterpart of ASTM D3518; ISO's coupon is 25 mm × 250 mm × 2 mm) with gauges along and across it. Then τ12 = load/(2 × area) and γ12 = εx − εy, and G12 is the chord slope between γ12 = 0.001 and 0.005. E1 and E2 can be backed out of x and y tests on an unequal cross-ply such as [0₂/90]s. The coupon is not in pure shear, so ISO warns that its shear strength reads low.

Predict, then check

A carbon/epoxy [±45]2s coupon pulled to σx = 30 MPa reads εx = 1,556 µε and εy = −1,171 µε. What is G12?

Worked examples

Engineering constants of a cross-ply · Carbon/epoxy [0/90]2s, eight 0.125 mm plies, h = 1 mm
  1. A11 = A22 = 74,968 N/mm, A12 = 3,099 N/mm, A66 = 5,500 N/mm, A16 = A26 = 0
  2. Ex = (A11A22 − A12²)/(h·A22) = 74.84 GPa = Ey
  3. νxy = A12/A22 = 0.0413
  4. Gxy = A66/h = 5.5 GPa, exactly G12: 0° and 90° plies add nothing in shear
  5. Bending: Exf = 12/(h³d11) = 98.74 GPa, higher than Ex because a 0° ply is outside

Answer: Ex = Ey = 74.8 GPa, νxy = 0.041, Gxy = 5.5 GPa

Reducing a ±45 shear test · E-glass/epoxy [±45]4s coupon, 25 mm × 2 mm section (16 plies of 0.125 mm), load P = 2 kN; gauges read εx = 2,196 µε and εy = −1,234 µε (simulated readings)
  1. Area = 25 × 2 = 50 mm², σx = P/area = 40 MPa
  2. τ12 = P/(2 × area) = 20 MPa
  3. γ12 = εx − εy = 2,196 − (−1,234) = 3,430 µε
  4. G12 = τ12/γ12 = 20/0.00343 = 5.831 GPa
  5. For the chord, read the loads at γ12 = 0.001 and 0.005: 583 N and 2,915 N give τ12 = 5.83 and 29.15 MPa, slope 5.83 GPa

Answer: G12 = 5.83 GPa (the ply value is 5.83 GPa)

Backing E1 and E2 out of cross-ply tests · Carbon/epoxy [0₂/90]s (2/3 of the plies at 0°), coupons cut along x and along y, each pulled to 100 MPa (simulated)
  1. x coupon: εx = 1,040.7 µε, εy = −60.1 µε, so Ex = 96.089 GPa and νxy = 0.0578
  2. y coupon: εy = 1,866.8 µε, so Ey = 53.569 GPa
  3. Invert the measured compliance [[1/Ex, −νxy/Ex], [−νxy/Ex, 1/Ey]]: A11/h = 96,268, A22/h = 53,669, A12/h = 3,099 MPa
  4. A11/h = (2/3)Q11 + (1/3)Q22 and A22/h = (1/3)Q11 + (2/3)Q22 give Q11 = 138,868 and Q22 = 11,069 MPa; Q12 = A12/h
  5. E1 = Q11 − Q12²/Q22 = 138 GPa, E2 = Q22 − Q12²/Q11 = 11 GPa, ν12 = Q12/Q22 = 0.28
  6. Quick estimate ignoring Poisson: E1 ≈ 2Ex − Ey = 138.6 GPa, E2 ≈ 2Ey − Ex = 11.05 GPa

Answer: E1 = 138 GPa, E2 = 11 GPa, ν12 = 0.28; a [0/90]s alone could not do it (Ex = Ey)

Chapter 21

Lamina strength: the maximum stress and maximum strain criteria

Which syllabus covers thisAU CME382 Unit IIIVTU not in syllabusSPPU not in syllabusMU MEDLO8051 Module 3KTU not in syllabus

Which strengths describe a unidirectional lamina?

Five numbers, all measured on the material axes: Xt and Xc along the fibres in tension and compression, Yt and Yc across them, and the in-plane shear strength S. For carbon/epoxy T300/914C they are 1500, 900, 27, 200 and 80 MPa. Along the fibres the lamina is about 56 times stronger than across them, where only the epoxy and the fibre-matrix bond carry load. Compression along the fibres is lower than tension because fibres buckle on a tiny scale (kinking). On the material axes the sign of shear does not matter.

How does the maximum stress criterion work, and why does off-axis strength fall so fast?

Turn the applied stresses into σ1, σ2 and τ12 and compare each with its own strength. The ply fails when any one reaches its limit, and that names the mode. Pull a carbon/epoxy ply along x with its fibres at θ: the fibres fail at Xt/cos²θ, shear at S/(sinθ cosθ) and the matrix at Yt/sin²θ. Fibres govern only up to 3.05°, shear up to 18.65°, then the matrix. At 30° the ply fails at 108 MPa, 7.2% of its strength along the fibres.

Off-axis strength of a unidirectional lamina: maximum stress and maximum strain, fibre, shear and transverse failure modes: interactive loads as you scroll

How is the maximum strain criterion different?

It compares ε1, ε2 and γ12 with ultimate strains, here taken as strength divided by modulus (linear to failure). The difference comes only from Poisson's ratio: a stress along one axis also strains the other. For the carbon ply at 30° it gives 115.8 MPa against 108 MPa by maximum stress. The gap can be large. Squeeze glass/epoxy LY556 along its fibres and the Poisson bulge across them reaches the transverse tensile strain at 380 MPa, well below Xc = 570 MPa. With ν12 = 0 the two criteria agree exactly.

What is a strength ratio, and why does the sign of shear matter off-axis?

The strength ratio R is the factor by which every applied stress can be multiplied before failure. R = 1.5 means 50% margin; R below 1 means the ply has already failed. In the interactive, the 30° carbon ply at |σx| = 100 MPa has R = 1.08. Add a shear τxy = σx/2 and the result depends on its sign. With +τxy, σ2 turns into compression and R = 4.37. With −τxy, σ2 becomes a large tension and R = 0.395. On the material axes shear sign is irrelevant, but off-axis it decides σ2.

Predict, then check

A carbon/epoxy ply (Xt = 1500, Yt = 27, S = 80 MPa) with fibres at 10° to x is pulled along x. By maximum stress, what fails first?

Worked examples

Off-axis tension of a glass/epoxy ply · E-glass/epoxy LY556 ply (Xt = 1140, Yt = 35, S = 72 MPa), fibres at 20° to x, pulled by σx alone
  1. cos²20° = 0.883, sin²20° = 0.117, sin20° cos20° = 0.3214
  2. Fibre limit: 1140/0.883 = 1291 MPa
  3. Matrix limit: 35/0.117 = 299.2 MPa
  4. Shear limit: 72/0.3214 = 224 MPa
  5. Lowest: in-plane shear. The switch angles are atan(S/Xt) = 3.61° and atan(Yt/S) = 25.92°, and 20° lies between them

Answer: σx = 224 MPa, in-plane shear failure (the matrix limit, 299 MPa, is close behind)

Strength ratio for a ply in a drone arm · Carbon/epoxy T300/914C ply at 45° in a drone arm; an FE run gives σx = 40, σy = 10, τxy = −15 MPa (illustrative)
  1. At 45°: σ1 = (σx + σy)/2 + τxy = 25 − 15 = 10 MPa
  2. σ2 = (σx + σy)/2 − τxy = 25 + 15 = 40 MPa; τ12 = −(σx − σy)/2 = −15 MPa
  3. Ratios: fibre 1500/10 = 150, matrix 27/40 = 0.675, shear 80/15 = 5.33
  4. The smallest, R = 0.675, is below 1: the matrix has already cracked, parallel to the fibres

Answer: R = 0.675 in transverse tension: fails (needs about 1.48× more matrix strength or a different angle)

When maximum strain and maximum stress disagree · E-glass/epoxy LY556 ply, σ1 = −450 MPa along the fibres, σ2 = τ12 = 0; E1 = 53.48 GPa, E2 = 17.7 GPa, ν12 = 0.278
  1. Maximum stress: R = Xc/450 = 570/450 = 1.267, safe
  2. Strains: ε1 = −450/53480 = −8414 µε; ε2 = +ν12 × 450/E1 = 2339 µε (the ply bulges across)
  3. Transverse tensile strain limit = Yt/E2 = 35/17700 = 1977 µε
  4. Maximum strain: R = 1977/2339 = 0.845, fails by transverse tension strain

Answer: Max stress R = 1.27 (safe), max strain R = 0.85 (fails): the Poisson term decides

Chapter 22

Interactive criteria: von Mises, Hill, Tsai-Hill and Tsai-Wu

Which syllabus covers thisAU CME382 Unit IIIVTU not in syllabusSPPU not in syllabusMU MEDLO8051 Module 3KTU not in syllabus

Where do the interactive criteria come from?

Von Mises wrote one equation for yielding of an isotropic metal: in plane stress, σ1² − σ1σ2 + σ2² = σY². Every stress component counts towards the same limit, so no single component has to reach σY. Rodney Hill in 1948 extended this to anisotropic metals such as rolled sheet, with a different yield stress in each direction. Azzi and Tsai (1965) put the five composite strengths into Hill's form, giving Tsai-Hill. These criteria predict whether a ply fails, but not which mode, unlike maximum stress.

How does Tsai-Hill combine the stresses?

It adds the squared stress-to-strength ratios and subtracts an interaction term. X and Y are chosen by the sign of σ1 and σ2, so the envelope is four pieces of ellipse. In the interactive the carbon ply carries σ1 = 750, σ2 = 9 and τ12 = 28 MPa. Each is at most half its own strength, so maximum stress gives R = 2. Tsai-Hill adds these shares together and gives R = 1.442.

What does Tsai-Wu add?

Linear terms. F1σ1 + F2σ2 + F11σ1² + F22σ2² + 2F12σ1σ2 + F66τ12² = 1 gives one smooth ellipse, and the linear terms shift it towards the side with the higher strength. For carbon F2 = 1/Yt − 1/Yc = 0.032 per MPa, so transverse tension uses up strength quickly. F12 needs equal biaxial tests, which are very hard to run, so Tsai's estimate −½√(F11F22) is used. The ellipse stays closed while F11F22 exceeds F12². At the interactive's default point Tsai-Wu gives R = 1.499.

Failure envelopes in fibre and transverse stress: maximum stress, maximum strain, Tsai-Hill and the Tsai-Wu ellipse: interactive loads as you scroll

How do you get a strength ratio from Tsai-Wu, and where should you distrust it?

Multiply every stress by R and set the index to 1. The squared terms grow as R² and the linear terms as R, so R is the positive root of aR² + bR − 1 = 0. The index itself is not a load factor: at the default point it is 0.43, which looks like room to double the load, yet R = 1.5, so the load can grow by only 50%. With F12* = −0.5 the carbon ellipse reaches σ1 = −2646 MPa under transverse compression, far beyond Xc = 900 MPa. No test supports that, so check stress states in that corner with another criterion.

Predict, then check

A carbon/epoxy ply carries σ1 = Xt/2, σ2 = Yt/2 and τ12 = S/2, all positive. Maximum stress gives R = 2. What does Tsai-Hill give?

Worked examples

Tsai-Hill for a wind-blade spar cap ply · E-glass/epoxy LY556 ply in a spar cap: σ1 = 400, σ2 = −30, τ12 = 25 MPa (illustrative); Xt = 1140, Yc = 114, S = 72 MPa
  1. σ1 > 0 so X = Xt = 1140; σ2 < 0 so Y = Yc = 114
  2. (400/1140)² = 0.1231; −σ1σ2/X² = +0.0092
  3. (30/114)² = 0.0693; (25/72)² = 0.1206
  4. Index = 0.3222, R = 1/√0.3222 = 1.762
  5. Maximum stress for comparison: R = 2.85 (shear)

Answer: Tsai-Hill R = 1.76, safe, but 38% lower than maximum stress gives

Tsai-Wu for the same ply · Same stresses; Tsai-Wu with F12* = −0.5
  1. F1 = 1/1140 − 1/570 = −8.772×10⁻⁴; F2 = 1/35 − 1/114 = 19.799×10⁻³ per MPa
  2. F11 = 1.5389×10⁻⁶, F22 = 2.506×10⁻⁴, F66 = 1.929×10⁻⁴, F12 = −9.82×10⁻⁶ per MPa²
  3. Quadratic part a = 0.828, linear part b = −0.9449; index = a + b = −0.1168
  4. R from aR² + bR − 1 = 0: R = (−b + √(b² + 4a))/(2a) = 1.809

Answer: Tsai-Wu R = 1.81 (Tsai-Hill 1.76): the compressive σ2 helps here through the negative linear term F2σ2

How much does F12 matter? · Carbon/epoxy T300/914C ply under σ1 = 1000 MPa and σ2 = −150 MPa, τ12 = 0 (illustrative biaxial state)
  1. Maximum stress: R = min(1500/1000, 200/150) = 1.333
  2. Tsai-Hill (X = Xt, Y = Yc): R = 0.965
  3. Tsai-Wu with F12 = 0: R = 1.235
  4. Tsai-Wu with F12* = −0.5: R = 0.946

Answer: F12 = 0 says safe (R = 1.23), F12* = −0.5 says it fails (R = 0.95): in this tension-compression quadrant the untested F12 decides the verdict

Chapter 23

Laminate failure: first-ply failure, ply discount and last-ply failure

Which syllabus covers thisAU CME382 Unit IIIVTU not in syllabusSPPU not in syllabusMU not in syllabusKTU not in syllabus

What is first-ply failure, and how is it found?

Solve the laminate once for a unit load, say Nx = 1 N/mm. That gives every ply's σ1, σ2 and τ12, and the criterion gives each ply's strength ratio, which is also its failure load in N/mm. The smallest is the first-ply failure (FPF) load. For a 0.5 mm [0/90]s carbon/epoxy laminate under Nx, Tsai-Wu gives FPF = 91.9 N/mm, an average stress of 184 MPa. The 90° plies crack parallel to their fibres. The laminate is cracked, not broken.

What happens after the first ply fails?

In the ply-discount model used here, a ply that fails in a matrix mode keeps its fibres, but its E2 and G12 drop to almost zero. A fibre failure removes E1 as well. The laminate is solved again and the next failure found. The [0/90]s laminate cracks at 91.9 N/mm, then its 0° plies carry the load until their fibres break at 375 N/mm. That is the last-ply failure (LPF), 4.08 times FPF. Under constant load the strain jumps at each failure, giving the knee in the curve.

Loading a laminate to failure: first-ply failure, discounting failed plies and the last-ply failure load: interactive loads as you scroll

Which load do designers use, FPF or LPF?

It depends on what a matrix crack costs. In a pipe, tank or pressure vessel a crack can let liquid weep through and lets moisture in, so the design stays below FPF. In a dry structure the cracks may be tolerable, and ultimate strength is closer to LPF. In this model the [0/±45/90]s carbon laminate goes from 134 to 515 N/mm. A [±45]s laminate collapses at FPF (64.8 N/mm), because ±45 fibres alone cannot carry Nx when nothing holds the y direction. Real [±45]s coupons stretch a long way in nonlinear shear before they break.

What does the simple ply-discount model leave out?

Several effects, pulling both ways. Curing leaves tension across the fibres before any load is applied (chapter 24). A thin ply held between others resists transverse cracking better than a unidirectional test coupon suggests (the in-situ effect). Shear is not linear up to failure. The free edges of a coupon can delaminate early. Real stiffness falls step by step as cracks build up, not all at once. So treat FPF and LPF from this model as a first estimate, and check them against coupon and element tests.

Predict, then check

A 0.5 mm [0/90]s carbon/epoxy laminate pulled along x cracks its 90° plies at Nx = 92 N/mm. Roughly what load breaks it?

Worked examples

First-ply failure of a glass/epoxy bus panel skin · [0/90]s E-glass/epoxy LY556, a typical 0.125 mm ply (h = 0.5 mm), in-plane load Nx; maximum stress criterion
  1. A11 = 18262, A12 = 2525, A22 = 18262 N/mm (A16 = A26 = 0)
  2. For Nx = 1 N/mm: εx = 55.825 µε, εy = −7.718 µε
  3. 0° ply: σ1 = 3.0249 MPa, σ2 = 0.1417 MPa per N/mm
  4. 90° ply: σ1 = −0.1417 MPa, σ2 = 0.9751 MPa per N/mm
  5. 90° plies reach Yt = 35 MPa first: Nx = 35/0.9751 = 35.89 N/mm

Answer: FPF = 35.9 N/mm (average stress 72 MPa), 90° plies crack

Last-ply failure of the same skin · Discount the cracked 90° plies (E2, G12 to almost zero), re-solve, repeat
  1. Laminate modulus falls from Ex = 35.83 GPa to 27.26 GPa once the 90° plies have cracked
  2. Next, the 0° plies crack along their fibres at Nx = 126.6 N/mm (σ2 tension caused by the Poisson mismatch with the 90° fibres)
  3. Only the fibres are left. The 0° fibres reach Xt = 1140 MPa at Nx = 1140 × 0.25 = 285 N/mm
  4. LPF/FPF = 285/35.9 = 7.94

Answer: LPF = 285 N/mm, about 7.9 × FPF

First-ply failure of a quasi-isotropic drone-arm laminate · [0/±45/90]s carbon/epoxy T300/914C, 8 plies of 0.125 mm (h = 1 mm), Nx; Tsai-Wu with F12* = −0.5
  1. Per N/mm: 0° ply σ1 = 2.548, σ2 = −0.0054 MPa
  2. +45° ply σ1 = 0.909, σ2 = 0.0907, τ12 = −0.1327 MPa
  3. 90° ply σ1 = −0.7291, σ2 = 0.1869 MPa
  4. Tsai-Wu ratios (N/mm): 0° 598, ±45° 278, 90° 134.3
  5. Lowest: the 90° pair, FPF = 134.3 N/mm = 134 MPa average

Answer: FPF = 134 N/mm (90° plies); the ply-discount model then gives LPF = 515 N/mm

Chapter 24

Thermal analysis: lamina and laminate CTEs, residual stresses and zero-CTE laminates

Which syllabus covers thisAU CME382 Unit IVVTU not in syllabusSPPU not in syllabusMU not in syllabusKTU not in syllabus

How do the fibre and matrix set a lamina's expansion?

Along the fibres the stiff fibres hold the soft epoxy back, so α1 is a stiffness-weighted average (Schapery). T300 fibres even shrink slightly along their length when heated (α = −0.7 µε/°C), so T300/914C at Vf = 0.6 gives α1 = −0.06 µε/°C; the measured value is −1. Across the fibres the epoxy dominates, and it also bulges because it is held back axially: α2 = 36.8 predicted against 26 measured. At low Vf, α2 even exceeds the epoxy's own 55.

Thermal expansion of laminae and laminates, a zero-expansion angle-ply, residual stress after curing and warping: interactive loads as you scroll

How does temperature enter Hooke's law and laminate theory?

Only the mechanical strain, total strain minus αΔT, produces stress, so a ply that is free to expand carries no stress. In a laminate the plies want to expand by different amounts. Each ply's Q̄αΔT summed through the thickness gives the thermal resultants N_T and M_T, which act like extra loads. For a symmetric laminate the free expansion is A⁻¹N_T per degree. For a [0/90]s carbon/epoxy laminate that gives αx = 1.45 µε/°C, between the ply values of −1 and 26 but close to the stiff fibres.

How can a laminate have zero or even negative expansion?

Heating makes each ply swell across its fibres. In a [±θ]s carbon laminate the stiff ±θ fibres act like a pair of scissors with a very large Poisson's ratio: the swelling opens them in y and pulls them shut in x. At θ = 30.2° this gives αx = −4.49 µε/°C, and αx is exactly zero at ±43.2°. Glass fibres are not stiff enough: glass/epoxy never goes below 7.77. NASA notes that Hubble, JWST and WFIRST rely on carbon composite structures designed for near-zero expansion. A quasi-isotropic laminate expands equally in every in-plane direction.

Why does curing leave stresses and warping?

HexPly 914 cures at 175 °C. Assume the resin locks the plies together there; cooling to 20 °C is then ΔT = −155 °C. In [0/90]s T300/914C every ply ends up with σ2 = +40.9 MPa before any load, above the measured Yt of 27 MPa. This is an upper estimate: the resin relaxes while hot, and embedded plies are stronger than a test coupon. A two-ply [0/90] strip bends to a radius of 66 mm. Theory predicts a saddle, but Hyer (1981) showed that thin square plates snap to a cylinder. Hence symmetric layups.

Predict, then check

A two-ply [0/90] carbon/epoxy strip is cured flat at 175 °C. What does it look like at room temperature?

Worked examples

Lamina CTEs of glass/epoxy from its constituents · E-glass fibre (E = 80 GPa, α = 4.9 µε/°C, ν = 0.2) in LY556 epoxy (E = 3.35 GPa, α = 58, ν = 0.35), Vf = 0.55
  1. α1 = (80 × 4.9 × 0.55 + 3.35 × 58 × 0.45)/(80 × 0.55 + 3.35 × 0.45) = 303.04/45.5075 = 6.659 µε/°C
  2. ν12 = 0.2 × 0.55 + 0.35 × 0.45 = 0.2675
  3. α2 = (1 + 0.2) × 4.9 × 0.55 + (1 + 0.35) × 58 × 0.45 − 6.659 × 0.2675 = 36.69 µε/°C

Answer: α1 = 6.66, α2 = 36.7 µε/°C: the lamina expands 5.5 times more across the fibres

Thermal growth of a glass/epoxy bus panel · A 2 m long [0/90]s E-glass/epoxy LY556 side panel (0.125 mm plies) on a bus, between a 10 °C morning and a 50 °C afternoon in the sun (illustrative)
  1. A11 = 18262, A12 = 2525, A22 = 18262 N/mm
  2. Thermal resultants per °C: N_Tx = N_Ty = 0.2821 N/mm
  3. αx = (A⁻¹N_T)x = 13.57 µε/°C
  4. ΔL = αx × L × ΔT = 13.57×10⁻⁶ × 2000 mm × 40 = 1.09 mm

Answer: About 1.1 mm of growth, so the fixings need slotted holes or flexible bonding

Residual stress in a glass/epoxy cross-ply · [0/90]s E-glass/epoxy LY556 cured at 120 °C (illustrative) and cooled to 20 °C: ΔT = −100 °C
  1. Free strains: 0° ply αxΔT = −860 µε, 90° ply −2640 µε along x
  2. Laminate strain εx = εy = −1357 µε, between the two
  3. The 0° ply is made to shrink more than it wants along its fibres: σ1 = −20.8 MPa; across them (y) it is held back from shrinking: σ2 = +20.8 MPa
  4. σ2/Yt = 20.8/35 = 59% of the transverse strength is used before any load

Answer: σ2 = +20.8 MPa in every ply (59% of Yt), σ1 = −20.8 MPa

Chapter 25

Laminated plates: bending, buckling and free vibration

Which syllabus covers thisAU CME382 Unit VVTU not in syllabusSPPU not in syllabusMU not in syllabusKTU not in syllabus

What sets the bending stiffness of a laminated plate?

The [D] matrix. Each ply adds its Q̄ times (z³ at its bottom minus z³ at its top)/3, so plies far from the mid-plane count most. A 16-ply, 2 mm carbon/epoxy [0/90]4s plate has D11 = 57,966 N·mm but D22 = 41,992 N·mm, although it holds eight plies each way: its outermost plies are 0°. Flip it to [90/0]4s and the two swap. A specially orthotropic plate has D16 = D26 = 0; a [±45]4s plate does not, so bending also twists it slightly.

How does the Navier series give the deflection of a simply supported plate?

Write the pressure and the deflection as double sine series. Each sine already satisfies the simply supported edges, and for a specially orthotropic plate each term solves the plate equation on its own, so w is a sum of terms 16q/(π⁶ m n Dmn) over odd m and n. In the interactive ([0/90]4s, 300 × 200 mm, 1 kPa, illustrative) the centre deflects 0.421 mm; the first term alone gives 102.3 % of it. With D16 and D26 not zero the terms couple and the series is only approximate.

A laminated plate: deflection under pressure, the buckling load and mode, and natural frequencies with their mode shapes: interactive loads as you scroll

How does a laminated plate buckle under in-plane compression?

It bows into m half-waves along the load and one across, and m is whichever gives the lowest load. A 300 × 200 mm [0/90]4s plate buckles at 34.3 N/mm with m = 1. As the plate gets longer, m steps up: the change from one to two half-waves comes at a/b = 1.53. On a square plate [0]16 and [0/90]4s buckle at the same 29.3 N/mm, because only D11 + D22 enters there. A long plate approaches 2√(D11D22) + 2(D12 + 2D66), times π²/b².

What decides a plate's natural frequencies?

Stiffness against mass: ω = π²·√(Dmn/ρh), with the same Dmn as in the Navier deflection. The 300 × 200 mm, 2 mm [0/90]4s plate at ρ = 1.54 g/cm³ (an estimate) has f11 = 176 Hz. Mode (m, n) has m − 1 and n − 1 nodal lines. Carbon gives high frequencies because its stiffness per kilogram is high. If a motor, rotor or road input runs near a natural frequency, the panel resonates. The usual fixes are a stiffer layup, smaller panels or a sandwich core.

Predict, then check

A square, simply supported carbon/epoxy plate is laid up [0/90]4s, then the same plies are stacked [90/0]4s. Under the same pressure, which deflects less at the centre?

Worked examples

Bending stiffnesses of a 1 mm cross-ply · Carbon/epoxy T300/914C, [0₂/90₂]s, 8 plies of a typical 0.125 mm (h = 1 mm): find D11 and D22
  1. Q11 = E1/(1 − ν12ν21) = 1,38,868 MPa, Q22 = 11,069 MPa
  2. 0° plies sit at 0.25 ≤ |z| ≤ 0.5 mm, both halves: (2/3)(0.5³ − 0.25³) = 0.07292 mm³
  3. 90° plies sit at |z| ≤ 0.25 mm: (2/3)(0.25³) = 0.01042 mm³
  4. D11 = 1,38,868 × 0.07292 + 11,069 × 0.01042 = 10,241 N·mm
  5. D22 = 11,069 × 0.07292 + 1,38,868 × 0.01042 = 2,254 N·mm

Answer: D11 = 10,241 N·mm, D22 = 2,254 N·mm: the outer 0° plies make it 4.5 times stiffer along x

Buckling of a stiffened-skin bay · A [0/90]4s carbon/epoxy bay, 300 mm long (load direction) × 150 mm wide, 2 mm thick, simply supported; D11 = 57,966, D22 = 41,992, D12 + 2D66 = 9,400 N·mm
  1. m = 1: Nx = π²/150²[D11(150/300)² + 2(D12 + 2D66) + D22(300/150)²] = 88.3 N/mm
  2. m = 2: (mb/a) = 1, Nx = 52.1 N/mm
  3. m = 3: (mb/a) = 1.5, Nx = 73.6 N/mm
  4. The lowest is m = 2: two half-waves along the bay
  5. Average compressive stress at buckling = 52.1/2 = 26 MPa

Answer: Nx,cr = 52 N/mm in two half-waves, about 26 MPa, far below the lamina strengths: stability, not strength, sizes this skin

Is a panel clear of a 120 Hz drive? · A 250 × 250 mm [0/90]4s carbon/epoxy panel, 2 mm, simply supported, ρ = 1.54 g/cm³ (estimate); a motor at 120 Hz (illustrative)
  1. ρh = 1.54 × 10⁻⁹ t/mm³ × 2 mm = 3.08 × 10⁻⁹ t/mm²
  2. D11 = 57,966, D22 = 41,992, D12 + 2D66 = 9,400 N·mm
  3. D11(1/a)⁴ + 2(D12 + 2D66)(1/a)²(1/b)² + D22(1/b)⁴ = 30.402 × 10⁻⁶ N/mm³
  4. ω11 = π²√(30.402 × 10⁻⁶/3.08 × 10⁻⁹) = 981 rad/s, f11 = 156.1 Hz
  5. Next modes: (2,1) 463 Hz, (1,2) 406 Hz

Answer: f11 = 156 Hz, 30 % above the drive: clear, but a thin margin; a smaller or stiffer panel would add more

Chapter 26

Sandwich panels: faces, core, stiffness per kilogram and failure modes

Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302052-A Unit 6MU not in syllabusKTU not in syllabus

Why does a sandwich panel give so much stiffness per kilogram?

It works like an I-beam: two thin, stiff faces carry the bending as tension and compression, and a light core holds them apart and carries the shear. Bending stiffness grows with the square of the face spacing d. Faces of 0.5 mm carbon/epoxy [0/±45/90]s on a 20 mm Rohacell 51 foam core give D = 5,735 N·m per metre width at 2.54 kg/m². A solid laminate of the same mass is 1.65 mm thick and 283 times less stiff.

Why does a sandwich beam deflect more than simple bending theory predicts?

The soft core shears. The deflection has two parts: bending, PL³/(48D) for a central load, and core shear, PL/(4U) with U = Gc d²/c. In the default interactive beam (50 mm wide, 400 mm span) shear is already 49 % of the deflection. On a 150 mm span with a 50 mm core it is 95 %. That is why sandwich specimens are tested on two spans to separate D and U. For a shear-dominated beam, a stiffer core helps more than thicker faces.

Sandwich panels: faces apart on a light core, stiffness and weight against a solid laminate, and which failure comes first: interactive loads as you scroll

How can a sandwich panel fail?

There are three main checks. Face failure: the face stress M/(t d b) reaches the face laminate's strength. Core shear: V/(d b) reaches the core shear strength, 0.8 MPa for Rohacell 51. Face wrinkling: the compressed face buckles into the core at about 0.5(Ef Ec Gc)^(1/3); 0.5 is a design value for foam cores (theory gives 0.825). Long spans are governed by the faces or wrinkling, short spans by core shear. Core crushing under a point load and face-core debonding also need checks.

What cores are used, and where do sandwich panels appear?

Rigid foams such as Rohacell 51 (0.05 g/cm³, shear modulus 21 MPa), aluminium or aramid-paper honeycombs and end-grain balsa are the common cores. Glass or carbon faces are bonded or co-cured onto them. Typical uses are aircraft floors and control surfaces, wind-turbine blade shells, boat hulls, rail and bus interior panels, and drone bodies; an illustrative case is a Hosur shop making glass-faced foam panels for bus roofs. The weak points are bolted joints (they need inserts), local impact, and water getting into honeycomb cells.

Predict, then check

A sandwich has thin faces on a 20 mm core. You double the core to 40 mm and keep the same faces. Roughly what happens to the bending stiffness?

Worked examples

Stiffness and mass of a carbon-faced foam panel · Faces 0.5 mm carbon/epoxy [0/±45/90]s (Ex = 54.14 GPa from laminate theory, 1.54 g/cm³), core 20 mm Rohacell 51 (Ec = 70 MPa, 0.05 g/cm³)
  1. d = c + t = 20.5 mm
  2. Faces about the centre: Ef t d²/2 = 54,136 × 0.5 × 20.5²/2 = 56,87,692 N·mm
  3. Faces' own bending Ef t³/6 = 1,128 N·mm; core Ec c³/12 = 46,667 N·mm
  4. D = 57,35,487 N·mm per mm width = 5,735 N·m per metre; the thin-face formula is 0.83 % low
  5. Mass = 2 × 1.54 × 0.5 + 0.05 × 20 = 2.54 kg/m²
  6. Same mass as a solid laminate 1.649 mm thick: D = 54,136 × 1.649³/12 = 20,242 N·mm

Answer: D = 5,735 N·m at 2.54 kg/m², 283 times the same-mass solid laminate

Bending and shear deflection in a 3-point test · The panel of Example 1 cut as a beam 50 mm wide, span 400 mm, central load 500 N (illustrative); Gc = 21 MPa
  1. Bending: δb = PL³/(48 D b) = 500 × 400³/(48 × 57,35,487 × 50) = 2.325 mm
  2. Shear stiffness U = Gc d²/c = 21 × 20.5²/20 = 441.3 N per mm width
  3. Shear: δs = PL/(4 U b) = 500 × 400/(4 × 441.3 × 50) = 2.266 mm
  4. Total δ = 4.591 mm; core shear is 49 % of it

Answer: δ = 4.59 mm, of which 2.27 mm is core shear

Which failure comes first? · UD carbon/epoxy faces [0]8, 0.5 mm (Ef = 138 GPa, strength = Xc = 900 MPa on the compressed face), 20 mm Rohacell 51 core (τ = 0.8 MPa), beam 50 mm wide, 3-point bend
  1. Span 400 mm, M = PL/4, V = P/2, d = 20.5 mm
  2. Face: 900 = (P × 400/4)/(0.5 × 20.5 × 50), P = 4,612 N
  3. Core shear: 0.8 = (P/2)/(20.5 × 50), P = 1,640 N
  4. Wrinkling: σwr = 0.5 × (1,38,000 × 70 × 21)^(1/3) = 293.8 MPa, P = 1,506 N
  5. Lowest at 400 mm: wrinkling, 1,506 N
  6. Span 150 mm: face 12,300 N, wrinkling 4,015 N, core shear still 1,640 N: core shear governs

Answer: Face wrinkling at 1.51 kN on the 400 mm span; core shear at 1.64 kN on a 150 mm span

Chapter 27

Testing composites: tension, compression, flexure, short-beam shear, DCB and ENF

Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302052-A Units 4, 5MU not in syllabusKTU not in syllabus

How are tensile and compressive properties of a laminate measured?

ASTM D3039 pulls a straight-sided strip, usually with bonded end tabs, and reads strain with a gauge or extensometer. Strength is Pmax/(w h), and the modulus is the slope over a fixed strain window such as 1000 to 3000 µε. A 15 × 2 mm carbon/epoxy strip needs about 45 kN. Compression is harder because a slender coupon buckles first. ASTM D6641 grips the coupon in blocks that load it through the ends and by shear, leaving only about 13 mm free. A clamped Euler estimate puts the minimum carbon thickness for that length near 0.58 mm.

What do the flexure and short-beam shear tests measure?

Flexure (ASTM D7264) bends a beam on a span of 32 times its thickness. The outer-fibre stress is 3PL/(2bh²), and the modulus is L³m/(4bh³) from the load-deflection slope m. Some of the deflection is shear, so the apparent modulus of carbon at 32:1 comes out about 2.9 % below E1. The short-beam shear test (D2344) uses a span of only 4 h, so the beam fails by interlaminar shear: Fsbs = 0.75 Pmax/(b h). That value is apparent, not a pure shear strength. It is mainly used for quality control.

How are delamination toughnesses G_Ic and G_IIc measured?

A thin film moulded into the mid-plane starts a crack. In the double cantilever beam (DCB, D5528) the two arms are pulled apart (mode I), and G = 3Pδ/(2ba) from beam theory; the standard adds a small crack-length correction. In end-notched flexure (ENF, D7905) the cracked beam is bent so the crack faces slide (mode II). G comes from a compliance calibration C = A + m a³ and G = 3 m P² a²/(2b). With illustrative values (G_Ic 0.25 kJ/m²), a 2 mm, 25 mm wide carbon DCB with a 50 mm crack starts to grow at 26.8 N.

Composite tests: tension, compression, flexure, short-beam shear, DCB and ENF, from a load curve to the property: interactive loads as you scroll

What else goes into a composite test programme?

Specimens are cut from a panel made like the real part, checked for voids, measured at several points and conditioned (often hot and wet), because the matrix and the interface are sensitive to moisture. Each property is the mean of several specimens; one NASA mode II study averaged five per material source. Fatigue tests repeat the loading for millions of cycles. Ply adhesion (ASTM F904) and ISO equivalents such as ISO 14126 and ISO 15024 complete the set. The failure mode is reported along with the number: a tension coupon that breaks inside its tab gives an invalid result.

Predict, then check

The same carbon/epoxy flexure specimen is tested on a span of 16 times its thickness instead of 32. What happens to the apparent flexural modulus?

Worked examples

Tensile strength and chord modulus · Glass/epoxy UD strip 15 mm × 1.5 mm; readings: 1,203 N at 1000 µε, 3,610 N at 3000 µε, maximum load 25,650 N (illustrative)
  1. Area = 15 × 1.5 = 22.5 mm²
  2. Stresses: 53.48 MPa and 160.44 MPa
  3. Chord modulus = (160.44 − 53.48)/(3000 − 1000) × 10⁻⁶ = 53,480 MPa
  4. Strength = 25,650/22.5 = 1,140 MPa

Answer: E1 = 53.5 GPa, Xt = 1,140 MPa, matching the E-glass/LY556 lamina data

Short-beam strength and a flexure check · Carbon/epoxy UD, h = 3 mm; short beam 6 mm wide broke at 1,900 N (illustrative); a flexure beam 13 mm wide at 32:1
  1. Short-beam span = 4h = 12 mm, width 2h = 6 mm
  2. Fsbs = 0.75 × 1,900/(6 × 3) = 79.2 MPa (apparent interlaminar shear strength)
  3. Flexure span = 32 × 3 = 96 mm; to reach Xc = 900 MPa the load is P = 2σ b h²/(3L) = 731 N
  4. Check: σ = 3 × 731.2 × 96/(2 × 13 × 3²) = 900 MPa

Answer: Fsbs = 79 MPa; the flexure beam needs about 731 N to fail

G_Ic from one DCB reading · Carbon/epoxy DCB, 3 mm thick (arms 1.5 mm), 25 mm wide, crack a = 60 mm; reading P = 41 N at opening δ = 6.09 mm (illustrative)
  1. Beam theory: G = 3Pδ/(2ba) = 3 × 41 × 6.09/(2 × 25 × 60)
  2. = 0.2497 N/mm = 0.25 kJ/m²
  3. Check the compliance: δ/P = 0.1485 mm/N vs 8a³/(E1 b t³) = 0.1484 mm/N
  4. The standard corrects a to a + |Δ| from a plot of the cube root of compliance against a

Answer: G_Ic ≈ 0.25 kJ/m²

Chapter 28

Damage, inspection and repair: delamination, ultrasonic C-scan, thermography and scarf repair

Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302052-A Unit 5MU MEDLO8051 Modules 5, 6KTU not in syllabus

What kinds of damage does a laminate suffer, and why is impact the worry?

Matrix cracks form first, in plies loaded across their fibres. Delaminations open between plies at free edges, holes, ply drops and impacts. Fibres break under high tension or compression, and fibres can debond from the matrix. A dropped tool or hail can leave barely visible impact damage (BVID): a dent you can hardly see outside, and a cone of delaminations that widens with depth inside. Delaminations cut the compressive strength because the sub-laminates buckle separately. That is why impacted parts are inspected rather than judged by eye.

How does an ultrasonic C-scan find a delamination and its depth?

A probe sends a short pulse into the laminate. Echoes come back from the front face, from any gap such as a delamination, and from the back wall. Depth = v t/2, with t the round-trip time. Through-thickness sound speed in carbon/epoxy is about 2.9 mm/µs, so a 4 mm laminate gives a back-wall echo at 2.76 µs. A delamination 1.5 mm down echoes at 1.03 µs and hides the back wall. A C-scan moves the probe over a grid and colours each point by the depth of its first echo.

Damage and repair: delamination found by an ultrasonic C-scan, thermography, and a scarf repair's bondline stresses: interactive loads as you scroll

How does flash thermography show hidden damage?

A flash heats the surface, and an infrared camera watches it cool. Heat flows inward, but a delamination blocks it, so the patch above runs hotter. In a 1-D model the spot appears at about t = d²/(α ln 40). With an illustrative diffusivity of 0.42 mm²/s, a gap 1.5 mm deep shows after 1.5 s, and one twice as deep needs four times as long. Sideways heat flow blurs deep defects, so thermography suits thin skins. Radiography, shearography and acoustic emission complete the toolbox.

How is a damaged laminate repaired with a scarf?

The damage is cut out and the edge is ground into a shallow taper, ratio 1:n. The surface is cleaned and dried, and new plies matching the parent ones are laid in with film adhesive and cured. On a taper the bond line is loaded mainly in shear: τ = σ sinθ cosθ with θ = atan(1/n). At 300 MPa, a 1:30 taper gives 10 MPa but 1:10 gives 29.7 MPa. The cost is size: a 4 mm skin at 1:30 needs 120 mm of taper on each side. Bolted patches are quicker and less efficient.

Predict, then check

A scarf repair is redesigned from a 1:20 to a 1:40 taper. Roughly what happens to the shear stress in the bond line?

Worked examples

Locating a delamination by time of flight · A 5 mm carbon/epoxy skin (40 plies of a typical 0.125 mm), v = 2.9 mm/µs; an echo arrives 1.38 µs after the front-face echo, and the back-wall echo is missing
  1. Expected back wall: 2 × 5/2.9 = 3.45 µs
  2. Depth = v t/2 = 2.9 × 1.38/2 = 2 mm
  3. 2/0.125 = 16 plies down
  4. The missing back-wall echo means the gap reflects nearly all the sound: a delamination, not a small void

Answer: A delamination 2 mm deep, between plies 16 and 17

Sizing a scarf repair · A 3 mm skin (24 plies) with damage cleaned out to a 20 mm hole; taper 1:30
  1. Scarf length per side = 30 × 3 = 90 mm
  2. Repair diameter = 2 × 90 + 20 = 200 mm
  3. Each of the 24 plies steps back 90/24 = 3.75 mm
  4. Bond angle θ = atan(1/30) = 1.91°

Answer: A 200 mm repair with 3.75 mm per ply step

Bond-line stress and the steepest acceptable taper · Far-field stress 250 MPa in the skin; adhesive design allowable 20 MPa in shear (illustrative)
  1. 1:20: θ = 2.86°, τ = 250 sinθ cosθ = 12.47 MPa, σn = 250 sin²θ = 0.623 MPa
  2. 1:50: θ = 1.15°, τ = 5 MPa, σn = 0.1 MPa
  3. Limit: 250 sinθ cosθ = 20, so sin 2θ = 0.16, θ = 4.6°
  4. n = 1/tan θ = 12.4

Answer: τ = 12.5 MPa at 1:20 and 5 MPa at 1:50; any taper flatter than about 1:13 keeps τ within 20 MPa

Keep going

Recommended reading

  • Principles of Composite Material Mechanics, R. F. Gibson
  • Stress Analysis of Fiber-Reinforced Composite Materials, M. W. Hyer
  • Analysis and Performance of Fiber Composites, B. D. Agarwal, L. J. Broutman and K. Chandrashekhara
  • Engineering Mechanics of Composite Materials, I. M. Daniel and O. Ishai
  • Mechanics of Composite Materials, A. K. Kaw
  • Mechanics of Composite Materials, R. M. Jones
  • Fiber-Reinforced Composites: Materials, Manufacturing and Design, P. K. Mallick
  • Composite Materials: Science and Engineering, K. K. Chawla
  • Composite Materials, S. C. Sharma

How this book was made

Chapters follow the official syllabi listed above. Every interactive's formulas and every worked-example number were checked by script. Explanations, animations and examples are original to Skill-Lync.

From the exam to a core job

Talk to a counsellor.

Ask how CAE and composites engineers use composite materials on real projects, and what the Post Graduate Program in CAE covers.

Talk to a career counsellor

Free 20-minute call. We'll map the right course to where you want to work.

By submitting you agree to our Terms and Privacy Policy.

Talk to a career counsellor

Talk to a career counsellor

Free 20-minute call. We'll map the right course to where you want to work.

By submitting you agree to our Terms and Privacy Policy.