Welding Technology
Strike an arc, choose a process, follow the heat into the plate and the metallurgy it leaves, then keep the weld from cracking, distorting or failing inspection
24 chapters, 24 interactives, few words. This book covers welding technology from the arc to the inspection report: joint design, arc and power sources, metal transfer, gas welding and cutting, SMAW, SAW, GTAW and GMAW, plasma and electroslag, resistance, friction stir, explosive and ultrasonic welding, adhesive bonding, electron and laser beams, brazing and MIAB, cladding, heat flow, the heat-affected zone, weld solidification, hydrogen cracking and preheat, stainless and dissimilar joints, aluminium and other non-ferrous metals, distortion and residual stress, and defects with ultrasonic testing. One plate, one joint and one set of welding procedures run through the whole book, so the numbers in one chapter carry into the next.
- AUCME395Casting and Welding Processes
- VTUBME302Manufacturing Process (joining modules 4-5)
- SPPU302045-AAdvanced Forming and Joining Processes
- MU—No separate welding course in the Rev-2019 mechanical scheme
- KTUPEMET416Advanced Metal Joining Techniques
By Skill-Lync · Updated 24 Nov 2026 · 24 chapters · 24 interactives · free, no sign-up
Welding processes, joints, edge preparation and how much weld metal a groove needs
Which syllabus covers thisAU not in syllabusVTU BME302 Module 4 (joining processes: classification of welding)SPPU not in syllabusMU not in syllabusKTU not in syllabus
How are welding processes classified?
Ask three questions. What melts? In fusion welding the base metal melts (arc, gas, resistance, laser, electron beam). In solid-state welding nothing melts: friction, explosive, ultrasonic and diffusion welding join by pressure and heat below the melting point. In brazing and soldering only the filler melts. Is pressure used? Resistance and forge welding use it, an arc weld does not. What is the heat source? An arc, a flame, an electric current through the joint, a beam or friction. Every process in this book sits in one of those boxes.
What are the five basic joints, and what does each need?
Butt, lap, tee, corner and edge. A butt joint puts two plates edge to edge and gives the full strength of the plate if the weld goes all the way through, so thick plate needs a groove. Lap, tee and corner joints use fillet welds, which need no edge preparation. An edge joint is for thin sheet. The book's running joint is a butt joint in 20 mm plate: it is the one where the groove, and the 2.05 kg of weld metal it takes per metre, decide the cost.
Why prepare the edges, and how much weld metal does the groove take?
An arc cannot melt through 20 mm in one pass, so you bevel the edges to reach the root. The cost is metal. The book's single-V (60°, 2 mm gap, 2 mm root face) fills 227.1 mm² and the 2 mm cap adds 34.4 mm²: 261.4 mm² or 2.05 kg per metre (assumed cap). At a 30 mm² bead that is 9 passes and 25.6 min of arc per metre at the GMAW deposition rate. Open the angle to 90° and the metal rises by 60 %: the groove angle is a cost dial.
What do the welding positions 1G to 6G mean?
The number is the position and the letter is the joint: G for a groove weld, F for a fillet. 1 is flat, 2 horizontal, 3 vertical, 4 overhead. For pipe, 5G is a fixed horizontal pipe welded all round and 6G is a pipe fixed at 45°, the hardest test a welder sits. ISO 6947 uses letters: PA is flat (1G, 1F), PC is horizontal (2G), PE is overhead (4G), PF is vertical up and PG vertical down. Flat is the fastest and cleanest, so shops turn the job to flat whenever they can.
When does a double-V groove pay, and why do fabricators like it?
A double-V takes metal from both faces, so for the same angle, gap and root face it uses less: 175 mm² against 261 mm² in 20 mm, a saving of 33 %, or 8.5 min of arc per metre. On metal volume alone it wins from 6.8 mm upward. The second benefit is balance: the single-V metal centroid sits 4.3 mm above the mid-plane and pulls the plate into an angle, the double-V sits on it. The catch: you must turn the job over and back-gouge, which costs time that the metal count does not show.
The same 20 mm plate, same gap and root face. You open the single-V from 60° to 90°. How much more weld metal per metre?
The bevel triangle grows with tan(α/2): 0.577 at 60°, 1.0 at 90°. The fill goes from 227 to 364 mm², the cap widens too, and the total goes from 261 to 419 mm²: 60 % more weld metal, more passes and more distortion.
Worked examples
Weld metal in the book's joint · 20 mm E350 plate (assumed), single-V butt, included angle 60°, root gap 2 mm, root face 2 mm, 2 mm cap. GMAW fill at 9.5 m/min of 1.2 mm wire, 95 % efficiency. Find the area, mass per metre, passes and arc time.
- Groove depth h = 20 − 2 = 18 mm. Gap strip: 2 × 20 = 40 mm².
- Bevel triangles: h² tan 30° = 18² × 0.5774 = 187.1 mm². Fill = 227.1 mm².
- Top width = 2 + 2 × 18 × 0.5774 = 22.78 mm. Cap = ⅔ × (width + 3) × 2 = 34.4 mm².
- Total = 261.4 mm² = 261.4 × 10⁻⁶ m² × 7,850 kg/m³ = 2.05 kg per metre.
- Passes at 30 mm² each: 8.71 → 9. Deposition = 4.81 kg/h, so arc time = 2.052 / 4.81 × 60 = 25.6 min per metre.
Answer: 261.4 mm², 2.05 kg/m, 9 passes, 25.6 min of arc per metre.
Single-V against double-V · Same plate and joint settings, but a symmetric double-V (two 9 mm deep bevels, 2 mm root face in the middle, a cap on each face). A 6 m seam.
- Each bevel is (20 − 2)/2 = 9 mm deep: fill = 40 + 2 × 9² × 0.5774 = 133.5 mm².
- Top width = 2 + 2 × 9 × 0.5774 = 12.39 mm. Two caps = 2 × ⅔ × (12.39 + 3) × 2 = 41 mm².
- Total = 174.6 mm² = 1.37 kg/m, against 2.05 for the single-V: 86.9 mm² or 33 % less.
- On the 6 m seam: 12.3 kg against 8.2 kg, a saving of 4.1 kg and 51 min of arc time (turning and back-gouging not counted).
Answer: 174.6 mm² and 1.37 kg/m, 33 % less than the single-V.
What a wider groove costs · The same single-V, but the fitter opens the included angle from 60° to 90° (an assumed shop habit, to make access easy).
- tan 45° = 1: fill = 40 + 18² × 1 = 364 mm².
- Top width = 2 + 2 × 18 = 38 mm. Cap = ⅔ × (38 + 3) × 2 = 54.7 mm². Total = 418.7 mm².
- Against 261.4 mm²: +157.2 mm², which is +60 %. Weld mass 3.29 kg/m and 14 passes at 30 mm².
Answer: 60 % more weld metal, about 1.23 kg per metre extra.
The welding arc and power sources: arc characteristics, CC and CV sources, self-regulation and duty cycle
Which syllabus covers thisAU not in syllabusVTU BME302 Module 4 (manual metal arc welding, equipment)SPPU not in syllabusMU not in syllabusKTU not in syllabus
What is a welding arc, and where do the volts go?
An arc is a column of ionised gas, a plasma, carrying tens to hundreds of amperes between the electrode and the work. The voltage splits three ways: a drop at the cathode, a drop at the anode and the column between them, which grows with arc length. Measured cathode falls are about 13 V on a steel electrode. The book's model (assumed) uses 14 V for both falls and 2 V per mm of column: a 4 mm arc at 156 A reads 23.3 V. Coatings add potassium and sodium, which ionise easily and keep an AC arc alive.
What is arc blow and how do you cure it?
The welding current makes a magnetic field. When the field is lopsided, near a plate end, a ground clamp or a step in thickness, it pushes the arc sideways. That is arc blow: the arc wanders, spatter rises, and the bead goes crooked. It is mainly a direct-current problem. Cures: move the ground clamp to the far end, weld away from the clamp, use a shorter arc, tack the joint more often, or switch to alternating current so the field reverses 100 times a second on a 50 Hz supply.
Why does SMAW use a constant-current source and GMAW a constant-voltage one?
A drooping (constant-current) source holds the current almost steady while the arc length wobbles, which suits a hand-held stick. In the model a 1 mm shorter arc changes the current by only 7 A of 156 A. A flat (constant-voltage) source does the opposite: the same 1 mm gives +60 A of 171 A, 8 times more. With a steady wire feed that swing is a feature. A short arc draws more current, melts the wire faster and restores the arc length by itself. That is self-regulation.
What kinds of welding power source are there, and what is open-circuit voltage?
A transformer steps the mains down and gives AC. A rectifier adds diodes for DC. An inverter rectifies, chops at tens of kilohertz and steps down again, which makes it small and fast to control. A generator, driven by an engine, is used where there is no mains. Open-circuit voltage (OCV) is the no-load reading at the terminals. A stick machine has a high one, 50 to 90 V (assumed range), to strike and hold an arc, and that is why it is also the voltage that can shock you. The standards cap it.
What does duty cycle mean, and how do you work it out at another current?
Duty cycle is the share of a 10-minute window a machine may spend welding at its rated current without overheating. A 300 A machine at 60 % may weld 6 minutes in 10. Heating goes as I², so the permitted duty at another current is the rated duty times (rated current / actual current)². At 350 A that is 44 %, 4.4 minutes in 10. At 100 % the machine can deliver 232 A.
During GMAW the torch drifts and the arc gets 1 mm shorter. On a constant-voltage source with a steady wire feed, what happens?
A flat source holds the voltage, so a shorter arc (less voltage drop in the column) pulls the current up: +60 A here. The wire melts faster than it feeds, the tip burns back and the arc lengthens again. On the drooping source the same 1 mm moves the current by only 7 A, which is why it keeps a stick weld steady but cannot self-regulate.
Worked examples
Operating point on a drooping source · Assumed CC machine: open-circuit voltage 70 V, falling 0.30 V per amp (30 V per 100 A). Assumed arc: V = 14 + 2L + (100 + 25L)/I with L = 4 mm. Find the current and arc voltage.
- Source: V = 70 − 0.30 I. Arc at 4 mm: V = 22 + 200/I.
- Set equal and multiply by I: 0.30 I² − 48 I + 200 = 0.
- The larger root is the stable one: I = (48 + √(48² − 4 × 0.30 × 200)) / 0.60 = 155.7 A. The small root (about 4 A) is unstable.
- Arc voltage = 70 − 0.30 × 155.7 = 23.28 V: falls 14 V, column 8 V, tail 1.3 V.
Answer: 156 A at 23.3 V.
Self-regulation: CC against CV · Same arc and same torch drift: the arc shortens from 4 mm to 3 mm. CC machine as above; CV machine assumed 30 V at no load, falling 4 V per 100 A.
- CC at 3 mm: the root of 0.30 I² − 50 I + 175 = 0 is 163.1 A: ΔI = +7.4 A, 4.7 % of 156 A.
- CV at 4 mm: 170.7 A at 23.2 V. At 3 mm: 231.1 A at 20.8 V. ΔI = +60.4 A, 35.4 %.
- The CV machine moves the current 8.2 times as much for the same arc change: the extra current melts the wire faster and puts the arc length back.
Answer: CC: +7 A. CV: +60 A, about 8 times more.
Duty cycle at a heavier current · A 300 A machine rated at 60 % duty on a 10-minute cycle is used for a 350 A procedure (assumed).
- Permitted duty = 60 × (300/350)² = 44.1 %.
- In 10 minutes: 4.41 minutes welding, 5.59 minutes cooling.
- Continuous (100 %) current = 300 × √(60/100) = 232.4 A.
- Check with the published worked case: a 200 A, 60 % machine at 250 A gives 60 × (200/250)² = 38.4 %.
Answer: 44 % duty, about 4.4 min of arc in 10.
Electrode melting and metal transfer: short-circuit, globular, spray and pulsed modes
Which syllabus covers thisAU not in syllabusVTU BME302 Module 4 (gas metal arc welding)SPPU 302045-A Unit 5 (cold metal transfer)MU not in syllabusKTU not in syllabus
Why does the electrode melt, and where does the heat come from?
Two places. The arc heats the wire tip, where the electrons land. The current also heats the wire itself on its way through the stick-out, as I²R. The wire must absorb about 1,165 kJ per kg to reach 1,500 °C and melt (assumed average heat capacity). In the model, 1.2 mm wire at 260 A and 15 mm stick-out takes 1,300 W from the arc (an assumed 5 V) and 448 W from resistance: 26 % of the heat is made in the wire itself, before it reaches the arc.
How fast does the wire melt, and what wire feed balances it?
Melting rate MR = αI + βLI², the Lesnewich form: the first term is arc heating, the second resistive heating of the stick-out L. Published constants for steel were not found, so the book builds them from the heat balance. At 260 A and 15 mm that gives 191 mm³/s, a wire feed of 10.15 m/min, within 7 % of the 9.5 m/min assumed for the book's GMAW pass. The wire feed you set must equal this, or the arc length drifts until it does.
What does a longer stick-out do?
It adds resistance, so more of the melting is done by I²R. Stretch the stick-out from 15 to 20 mm at 260 A and the wire melts 8.5 % faster (10.15 to 11.01 m/min). With a fixed wire feed the source answers by lowering the current: the wire feed of 9.5 m/min needs 247 A at 15 mm but only 232 A at 20 mm. Less current means less penetration, which is why a wandering stick-out gives lack of fusion.
What are the transfer modes, and what forces move the metal?
In short-circuit transfer the drop touches the pool and the current pinches it off, many times a second: low heat, good for thin sheet. In globular transfer big drops, two to three wire diameters, fall by gravity, with spatter. In spray transfer a stream of fine drops about the wire diameter crosses the arc. The forces: gravity, surface tension holding the drop on, the electromagnetic pinch squeezing the neck, and plasma drag pulling the drop along. Pulsed GMAW (chapter 7) buys spray-like transfer at a lower mean current.
What sets the globular-to-spray transition current, and why does CO₂ not spray?
The pinch force µ0I²/4π grows with current; the surface tension force πDγ holds the drop. They balance at I = 2π√(γD/µ0). For a 1.6 mm wire that is 246 A, against the 240 to 255 A Kim and Eagar measured in argon. The same model gives 213 A for 1.2 mm (not measured: a model). A longer stick-out lowers it by about 2 A per mm. In carbon dioxide the arc root climbs up the drop and the plasma pushes it off the wire: repelled globular transfer at any current, so a pure CO₂ shield sprays no metal.
With 1.2 mm wire at 15 mm stick-out you raise the current from 160 A to 260 A. By what factor does the wire feed needed to match the melting rise?
The arc term is proportional to I (×1.63) and the resistive term to I² (×2.64). Together the wire feed goes from 5.6 to 10.1 m/min, a factor 1.8. The stick-out heating is only 18 to 26 % of the total, so it nudges the ratio above the current ratio without taking it to the square.
Worked examples
Wire feed from current · 1.2 mm steel wire, 260 A, 15 mm stick-out. Assumed: arc heating 5 V × I, resistivity of the hot wire 5 × 10⁻⁷ Ω·m, 11,64,600 J/kg to heat from 20 °C and melt (c = 620 J/kg·K, latent heat 247 kJ/kg). Find the wire feed.
- Wire area A = π × 0.6² = 1.131 mm². Resistance of the stick-out R = 5×10⁻⁷ × 0.015 / 1.131×10⁻⁶ = 6.63 mΩ.
- Heat: arc 5 × 260 = 1,300 W; resistive 260² × R = 448 W. Total 1,748 W.
- Mass melted = 1,748 / 11,64,600 = 5.4 kg/h (191 mm³/s).
- Wire feed = 191.2 / 1.131 = 169.1 mm/s = 10.15 m/min. The kernel's 9.5 m/min is 6.8 % lower: inside a ±15 % band.
Answer: 10.15 m/min (5.13 kg/h deposited at 95 %).
Current for a set wire feed · The same wire and model. The wire feeder is set to 9.5 m/min. What current does the arc settle at for stick-outs of 15 mm and 20 mm?
- Solve melting rate = feed: 9.5 m/min needs 179.1 mm³/s.
- At 15 mm stick-out the balance is reached at I = 246.7 A. (The kernel's procedure quotes 260 A for 9.5 m/min; the model needs 5 % less, well inside the ±15 % band.)
- At 20 mm the extra I²R lets the wire melt at a lower current: I = 232.1 A, which is 14.6 A less.
Answer: 247 A at 15 mm and 232 A at 20 mm.
Transition current and drop rate · Liquid steel surface tension 1.2 N/m (assumed). Pinch force µ0I²/4π equals the surface tension force πDγ at the transition. Find Ic for 1.6 mm and 1.2 mm wire, and the spray drop rate at 260 A for 1.2 mm.
- 1.6 mm: Ic = 2π√(1.2 × 1.6×10⁻³ / 4π×10⁻⁷) = 245.6 A. Kim and Eagar measured 240 to 255 A (255 A at 26 mm, 240 A at 33 mm): the model sits inside the band.
- 1.2 mm: Ic = 212.7 A at the 15 mm reference stick-out (model only, not measured).
- At 260 A the arc is above it: spray. Drop diameter ≈ wire diameter 1.2 mm, volume π × 1.2³ / 6 = 0.905 mm³.
- Drops per second = melting rate / drop volume = 191.2 / 0.905 = 211 per second.
Answer: Ic = 246 A (1.6 mm) and 213 A (1.2 mm); about 211 spray drops a second.
Gas welding and oxy-fuel cutting: flame chemistry, flame types and cutting
Which syllabus covers thisAU not in syllabusVTU BME302 Module 4 (gas welding: types, flame characteristics)SPPU not in syllabusMU not in syllabusKTU not in syllabus
What is in a gas welding set, and what is the safety rule for acetylene?
Two cylinders, oxygen and acetylene, each with a regulator that drops the pressure to a working value. Hoses run to a torch that mixes the gases. Flashback arrestors and non-return valves stop a flame running back up the hose. Acetylene is unstable under pressure, so the cylinder holds it dissolved in acetone in a porous mass. Draw it too fast and acetone comes out with the gas. The rule: not more than one tenth of the cylinder content an hour in intermittent use (1/7 is the general limit).
What are the two combustion zones, and what makes a flame neutral, carburising or oxidising?
The inner cone burns acetylene on cylinder oxygen alone: C₂H₂ + O₂ → 2CO + H₂, releasing 448 kJ per mole. The outer envelope burns the CO and H₂ on oxygen from the air: 2CO + H₂ + 1.5 O₂ → 2CO₂ + H₂O, another 852 kJ. Neutral is an O₂:C₂H₂ ratio of 1.04 to 1.14. Less gives a carburising flame with a feather of unburnt acetylene. More gives an oxidising flame. At 1.1 the air supplies 56 % of the oxygen the gas finally burns.
How much heat does each zone give, and how hot is the flame?
From the standard enthalpies of formation, Hess's law gives 447.8 kJ/mol in the inner cone and 851.8 in the outer envelope (water condensed). At 15 °C one mole of gas occupies 23.64 L, so that is 18,938 and 36,024 kJ per m³ of acetylene, matching TWI's 18,890 and 35,882 within 0.5 %. The cone carries only 34 % of the heat but is the hottest part, about 3,160 °C in oxygen for acetylene against 2,828 °C for propane.
What are leftward and rightward welding, and when is a gas flame used today?
In leftward welding the torch moves left with the filler rod ahead of it: the flame is pointed away from the finished weld and preheats the joint. It suits thin plate and open gaps. In rightward welding the torch moves right with the rod behind it and the flame points back at the finished weld, which cools slowly and keeps the pool deep: it suits thicker plate. Gas welding is slow and the whole plate heats, so arc welding has replaced it for production. It survives for sheet, thin tube, repair and field work where no power is available.
How does oxy-fuel cutting work, and why does it cut steel but not stainless steel, aluminium or cast iron?
The flame heats steel to its ignition temperature, 700 to 900 °C, far below its melting range. A jet of pure oxygen then burns the iron and the liquid oxide is blown out of the kerf. In 20 mm plate with an assumed kerf of 1.9 mm that is 298 g of iron per metre and at least 63 L of oxygen to turn it to FeO (84 L if Fe₃O₄), a minimum: torch consumption is higher. Stainless steel forms a refractory chromium oxide, aluminium melts before it ignites, and cast iron's graphite spoils the burn. They need powder, plasma or laser cutting.
A welder opens the oxygen valve on a neutral oxy-acetylene flame until the O₂:C₂H₂ ratio is 1.3. What flame has she made?
The neutral band is 1.04 to 1.14. At 1.3 the extra cylinder oxygen burns CO to CO₂ inside the cone, adding about 91 kJ per mole of acetylene (448 rises to 538). The cone shortens, the flame is the hottest of the three and it oxidises the weld pool: good for brazing some brasses, bad for steel.
Worked examples
Heat of the two zones · Standard enthalpies of formation (kJ/mol, NIST): C₂H₂ +226.73, CO −110.53, CO₂ −393.51, H₂O liquid −285.83. Find the heat of the inner cone and the outer envelope per mole and per m³ of acetylene at 15 °C.
- Inner cone: C₂H₂ + O₂ → 2CO + H₂. ΔH = 2(−110.53) − 226.73 = −447.79 kJ/mol. 447.79 kJ are released.
- Outer: 2CO + H₂ + 1.5 O₂ → 2CO₂ + H₂O(l). ΔH = 2(−393.51) + (−285.83) − 2(−110.53) = −851.79 kJ/mol.
- Check: the two add to 1,299.58 kJ/mol, the heat of burning acetylene to CO₂ and liquid water in one step (Hess).
- Molar volume at 15 °C = 8.3145 × 288.15 / 1,01,325 = 23.64 L. Inner: 18,938 kJ/m³; outer: 36,024 kJ/m³. TWI quotes 18,890 and 35,882.
Answer: 447.8 and 851.8 kJ/mol, or 18,938 and 36,024 kJ per m³.
Where the oxygen comes from · A welding torch burns 0.8 m³/h of acetylene (assumed) at a neutral setting of O₂:C₂H₂ = 1.1. Air is 21 % oxygen.
- Complete burning needs 1 + 1.5 = 2.5 mol O₂ per mol C₂H₂.
- Cylinder oxygen = 0.8 × 1.1 = 0.88 m³/h. Oxygen from the air = 0.8 × (2.5 − 1.1) = 1.12 m³/h, which is 56 % of the total.
- That oxygen is in 5.3 m³ of air an hour.
- Heat release = 0.8 × 54,963 / 3,600 = 12.2 kW, of which the inner cone gives 34 %.
Answer: 56 % of the oxygen comes from the air; the flame releases about 12.2 kW.
Oxygen to cut 20 mm and 40 mm plate · Steel plate cut by oxy-fuel. Kerf = 1.5 + 0.02 t mm (assumed). Iron burns to FeO (assumed oxide): Fe + ½O₂ → FeO. Iron 7,850 kg/m³, 55.845 g/mol; oxygen 23.645 L/mol at 15 °C.
- 20 mm: kerf 1.9 mm. Iron per metre = 1.9 × 20 × 1,000 mm³ = 38 cm³ = 298.3 g = 5.34 mol.
- Oxygen = ½ × 5.34 = 2.67 mol = 63.2 L per metre. For Fe₃O₄ it would be ⅔ per Fe: 84.2 L.
- 40 mm: kerf 2.3 mm, iron 722 g, oxygen 153 L per metre.
- Doubling the thickness multiplies the oxygen by 2.42, not 2, because the kerf widens too. These are minimums.
Answer: At least 63 L/m (20 mm) and 153 L/m (40 mm).
Shielded metal arc welding: electrode coatings, classification and electrodes per joint
Which syllabus covers thisAU not in syllabusVTU BME302 Module 4 (manual metal arc welding)SPPU not in syllabusMU not in syllabusKTU not in syllabus
How does shielded metal arc welding work, and what does the coating do?
A flux-coated steel rod and the plate carry the arc. The arc melts the core wire and some plate. The coating melts too and does five jobs: it burns to a gas shield, floats up as slag that protects and shapes the bead, stabilises the arc with easily ionised potassium or sodium, adds alloy, and carries deoxidisers. The book's assumed root pass (3.15 mm E7018, 22 V, 110 A, 2.0 mm/s, k 0.8) puts in 0.968 kJ/mm. The Manufacturing Processes book has a heat-input calculator for other settings.
Which coating type do you pick: cellulosic, rutile, basic or iron powder?
Cellulosic (E6010) burns to a lot of gas and digs deep, on DC electrode positive only: pipe roots. Rutile (E6013) gives a smooth, easy arc on AC or DC for sheet and general work. Basic low-hydrogen (E7016, E7018) gives the toughest, crack-resistant metal but must be kept dry. Iron-powder rutile (E7024) packs metal powder in the coating: a recovery near 150 % (assumed) for fast flat and horizontal fillets. E7018 carries 115 % recovery, so it deposits 115 g of weld metal for every 100 g of core wire melted.
How do you read an AWS E7018 or an IS 814 code?
AWS A5.1: E means electrode. 70 is the minimum tensile strength in ksi, 483 MPa. The third digit is the positions: 1 all, 2 flat and horizontal fillet. The last two digits are coating and current: 18 is low-hydrogen with iron powder, AC or DC electrode positive. IS 814:2004 codes the same ideas in letters and four digits. Its own example ER4211 reads: rutile, 410-540 MPa, 22 % elongation with 47 J at 0 C, all positions, DC either polarity and AC at 50 V open circuit. The interactive decodes both side by side.
Why do low-hydrogen electrodes need ovens, and what temperatures?
A basic coating soaks up moisture from air. Moisture puts hydrogen in the weld, and hydrogen cracks hard steel. Keep opened cans in a cabinet at 120 to 150 °C. If the rods were exposed, redry E7018 at 340 to 400 °C for one hour (Lincoln data). Cellulosic E6010 is the opposite: do not rebake it, the coating needs its moisture. IS 814 grades the result by diffusible hydrogen: H1 up to 15, H2 up to 10, H3 up to 5 ml per 100 g of weld metal. The Hydrogen cracking chapter shows what that does to preheat.
How many electrodes does a joint need, and how long does the arc burn?
Take the root and hot pass of the book's joint: 21.2 mm², 0.167 kg per metre. A 3.15 mm E7018, 350 mm long with a 50 mm stub, melts 18.4 g of core and deposits 21.1 g. That is 7.9 electrodes a metre, each burning 2.1 min, so 16.7 arc minutes. If the welder's operator factor (arc-on share of working time) is 30 %, assumed, that is 0.93 h per metre. Here A_w is the area in mm², R the recovery, d the core, L the length and s the stub, all in mm.
For the same root and hot pass you change from 3.15 mm to 4.0 mm electrodes, same length, stub and coating. How does the number of electrodes per metre change?
Core wire mass scales with d². (3.15/4.0)² = 0.62, so electrodes per metre fall from 7.9 to 4.9, 38 % fewer. A bigger rod also needs more current (150 A against 110 A, assumed), and the root pass would not fit through a 2 mm gap.
Worked examples
Read two classifications · A drawing calls for E7024 for a flat horizontal fillet. The mill's IS 814 certificate says ER4211.
- E7024: 70 ksi × 6.895 = 483 MPa minimum. Third digit 2 means flat and horizontal fillet only. Last digit 4 is iron-powder titanium (rutile): AC or DC.
- No vertical or overhead: E7024 is a shop electrode, not a site one.
- ER4211: R rutile. First digit 4: 410 to 540 MPa and 330 MPa yield. Second digit 2: 22 % elongation, 47 J at 0 °C.
- Third digit 1: all positions. Fourth digit 1: DC with either polarity, or AC with 50 V open-circuit voltage minimum.
Answer: E7024 is 483 MPa, flat and horizontal fillet; ER4211 is a rutile all-position rod, 410 to 540 MPa, 47 J at 0 °C.
Electrodes and arc time for the root and hot pass · The book's joint (20 mm, 60°, gap 2, face 2). Weld the lowest 6 mm with 3.15 mm × 350 mm E7018, 50 mm stub, 110 A, recovery 115 %, operator factor 30 % (assumed).
- Area = gap × 6 + 4² × tan 30° = 12 + 9.24 = 21.24 mm², so 0.167 kg per metre.
- Core melted = π × 3.15² ÷ 4 × 300 mm = 2,338 mm³ = 18.35 g. Weld metal = 18.35 × 1.15 = 21.11 g.
- Electrodes per metre = 166.7 g ÷ 21.11 g = 7.9, so 8 whole rods.
- Burn time = core mass ÷ melting rate. Assume these 6 mm go in as two passes at the kernel's 2 mm/s (assumed), which means 0.6 kg/h at 110 A, so each rod burns 127 s; 7.9 rods = 16.7 min, which is exactly two passes at 2 mm/s.
- At 30 % arc-on: 16.7 ÷ 60 ÷ 0.30 = 0.93 h per metre.
Answer: 7.9 electrodes and 16.7 arc minutes a metre, 0.93 h at 30 % arc-on.
The whole joint by stick welding · Fill and cap the whole joint (261.4 mm²) with 4.0 mm × 450 mm E7018, 50 mm stub, 150 A, operator factor 30 % (assumed). The kernel GMAW needs 25.6 arc minutes.
- Weld metal = 2.05 kg per metre = 2,052 g.
- One rod: core π × 4.0² ÷ 4 × 400 mm = 39.5 g, weld metal 45.4 g. Rods = 45.2.
- Burn time per rod = 200 s at 150 A, so arc time = 150 min per metre.
- At 30 % arc-on that is 8.4 h per metre, against 25.6 arc minutes for GMAW: 5.9 times the arc time before the slag-chipping.
Answer: About 45 rods and 150 arc minutes a metre: SMAW is for position work and root runs, not for filling a long seam.
Submerged arc welding: fluxes, basicity index, wire-flux combinations and tandem arcs
Which syllabus covers thisAU not in syllabusVTU BME302 Module 4 (submerged arc welding)SPPU not in syllabusMU not in syllabusKTU not in syllabus
How does submerged arc welding work and where is it used?
A bare wire is fed into a heap of granular flux. The arc burns under the flux, so there are no sparks and no arc light. Some flux melts into slag that shields and shapes the bead; the rest is reused. Wires run from 1.2 to 6.4 mm and currents from 150 to 1,600 A (TWI). The book's SAW procedure (4 mm wire, 32 V, 600 A, 500 mm/min, k 1.0) gives 2.304 kJ/mm, more than twice the GMAW pass. The limit: the flux must lie on the joint, so it is a flat and horizontal process.
What are fused and agglomerated fluxes, and what do fluxes do?
Fused flux is melted in a furnace, solidified and crushed into glassy grains: uniform, low in moisture, but hard to add alloy to. Agglomerated flux is powders bonded into granules, so makers can add deoxidisers and alloys, but it must be dried. By behaviour a flux is neutral (little change to the weld metal), active (adds Mn and Si) or alloying. Its jobs: help arc striking, form a protective slag, shield the pool, deoxidise it, and sometimes alloy it.
What is the basicity index and what does it tell you about the weld?
The basicity index is bases over acids in the flux, weight per cent, with MnO, FeO, Al2O3 and TiO2 counted at half. TWI's bands: acid 0.5 to 0.8, neutral 0.8 to 1.2, basic 1.2 to 2.5, highly basic 2.5 to 4.0. Eagar measured five commercial fluxes. Flux B (BI 0.61, acid) left 544 ppm oxygen in the weld; flux E (BI 2.98, highly basic) left 201 ppm. Higher basicity means cleaner metal and better notch toughness. Acid fluxes tolerate rust and give a smooth bead at speed.
How is a wire-flux combination classified?
The flux and wire are specified together because both change the weld metal. AWS A5.17 reads F7A2-EM12K as (secondary sources): flux, 70 ksi minimum tensile, as-welded, Charpy at −20 °F, wire EM12K (low carbon, medium manganese, killed). The ISO 14171-A example S 46 3 AB S2 reads: submerged arc, 460 MPa yield, 47 J at −30 °C, aluminate-basic flux (AB, from ISO 14174), wire S2 (about 1 % Mn). The flux letters name the chemistry: MS manganese-silicate, CS calcium-silicate, AR aluminate-rutile, FB fluoride-basic.
How do wire size, current and a second wire change deposition?
Deposition rises with current and, at the same current, with a thinner wire, because the stick-out heats resistively. Lincoln's figures (6.7 kg/h for 2.0 mm and 4.7 kg/h for 4.8 mm at 500 A; 8.3 kg/h for 4.0 mm at 700 A) fit a two-term model that gives 6.6 kg/h at 600 A with 4 mm wire. Add a trailing wire at 0.8 of the lead current (assumed) and it is about 11.7 kg/h. The book's whole joint then takes 18.7 arc minutes (one wire) or 10.5 (tandem), against 25.6 for GMAW. Strip SAW uses 0.5 mm strip, 15 to 240 mm wide, to clad large areas.
You must weld a low-temperature pressure vessel with SAW. Of the five commercial fluxes A to E that Eagar measured, which gives the least oxygen in the weld, and why?
Weld oxygen fell as basicity rose: B 544 ppm, D 536, A 270, C 208, E 201. Flux E has the highest BI (2.98) and the lowest oxygen. Low oxygen means fewer oxide inclusions and better notch toughness. The price: basic fluxes are fussier about drying and give a less glossy bead.
Worked examples
Basicity index of flux B · Flux B (Eagar's analysis, wt %): CaO 18.9, MgO 1.4, CaF2 4.5, MnO 11.5, FeO 1.0, SiO2 40.1, Al2O3 6.1, TiO2 16.2.
- Bases = 18.9 + 1.4 + 4.5 + ½ × (11.5 + 1.0) = 31.05.
- Acids = 40.1 + ½ × (6.1 + 16.2) = 51.25.
- BI = 31.05 ÷ 51.25 = 0.61: an acid flux (below 0.8).
- Eagar printed 0.6 for this flux. His own index without CaF2 is 0.52 (printed 0.52). The weld held 544 ppm oxygen, the highest of the five.
Answer: BI 0.61, acid, 544 ppm oxygen in the weld.
Swap silica for lime in flux D · Flux D: CaO 27.5, MgO 9.6, CaF2 3.9, MnO 0.3, FeO 0.2, SiO2 54.1, Al2O3 4.8, TiO2 0. A maker replaces 10 points of SiO2 with CaO.
- Before: bases = 27.5 + 9.6 + 3.9 + ½ × 0.5 = 41.25; acids = 54.1 + ½ × 4.8 = 56.5; BI = 0.73, acid.
- After: CaO 37.5, SiO2 44.1: bases = 51.25; acids = 46.5.
- BI = 1.1: now neutral (0.8 to 1.2).
- The oxide total is unchanged. Ten points of swap moved the flux one class; to reach the basic band (1.2) it would need more.
Answer: BI rises from 0.73 to 1.1, from acid to neutral.
Single wire or tandem for the book's joint · Fill the whole 261.4 mm² groove (2.05 kg per metre) with 4 mm wire. Lead wire 600 A. Compare single wire with tandem (trail 480 A, assumed), and with the kernel GMAW at 4.81 kg/h.
- Deposition: one wire 6.58 kg/h; trail wire at 480 A 5.15 kg/h; tandem 11.7 kg/h. (Model fitted to Lincoln's three figures; SAW taken as 100 % efficient, assumed.)
- Arc time, one wire = 2.05 kg ÷ 6.58 kg/h × 60 = 18.7 min per metre.
- Tandem = 2.05 ÷ 11.7 × 60 = 10.5 min.
- GMAW: 25.6 min. SAW is 1.37 times faster with one wire and 2.4 times faster in tandem.
- Each pass lays about 28 mm² at 500 mm/min, against 30 mm² for the GMAW pass. SAW wins on fewer starts, not just on raw speed.
Answer: 18.7 min (one wire) or 10.5 min (tandem) per metre, against 25.6 min for GMAW.
GTAW and GMAW: polarity, shielding gases, pulsed current and cold metal transfer
Which syllabus covers thisAU not in syllabusVTU BME302 Module 4 (gas tungsten arc and gas metal arc welding)SPPU 302045-A Unit 5 (cold metal transfer)MU not in syllabusKTU not in syllabus
How does GTAW work, and which tungsten electrode do you choose?
A non-consumable tungsten electrode strikes the arc, an inert gas shields it, and a separate filler rod is added by hand or machine. Pure tungsten is cheap and has limited use on AC aluminium. Thoriated tungsten starts and runs well but is slightly radioactive: dust is a health risk. Ceriated and lanthanated tungsten behave much the same and are not radioactive. The book's 304 pipe procedure (12 V, 120 A, 1.5 mm/s, k 0.6) puts in 0.576 kJ/mm, 41 % less than the 0.971 kJ/mm GMAW fill pass.
What do DCEN, DCEP and AC do to the weld?
DCEN (electrode negative) sends the electron heat into the work: a deep, narrow bead. Use it for steels, nickel and titanium. DCEP (electrode positive) heats the tungsten more and the work less: shallow, with a cleaning action that strips oxide, but it needs a fat electrode. AC alternates, so the half-cycle on EP cleans aluminium's oxide and the half on EN gives penetration. Balance control sets the time on each; the interactive uses 70 % EN as its AC default.
Which shielding gas for which job: argon, helium, CO2?
Ionisation energy is how hard it is to make a gas carry current: argon 15.8 eV, CO2 13.8, hydrogen 15.4, helium 24.6 (NIST). Argon strikes easily and runs at lower voltage. Helium needs more voltage, so the arc is hotter: used for thick aluminium and copper. CO2 and oxygen are active: they oxidise, so they go into steel mixes. The book's GMAW uses argon with 18 % CO2. Pure CO2 does not give true spray transfer.
How does pulsed GMAW give one small drop per pulse?
A high peak current Ip for a short time tp pinches one drop off, then a low background Ib keeps the arc alive. Steel data (Dutra: D = 236 A²s for a 1.0 mm wire) give about 340 A²s for the book's 1.2 mm wire, assumed by cross-section. Ip 400 A, tp 2.2 ms, Ib 60 A, 100 Hz gives Ip²tp = 352 A²s: one drop per pulse, 1.22 mm, about the wire size. Mean current is only 135 A and rms 195 A. A steady arc at that feed would be globular and spatter.
What are cold metal transfer and synergic control?
In cold metal transfer (CMT, developed by Fronius) the drop touches the pool, the machine sees the short circuit, drops the current and pulls the wire back. The drop is peeled off with almost no current, so heat input and spatter are low. It suits thin sheet, under 10 mm, and aluminium to steel joints. Synergic control means one knob, the wire feed speed, and the machine picks voltage, pulse peak and frequency from stored curves for that wire and gas.
A pulsed GMAW set-up gives one drop per pulse at 100 Hz (Ip 400 A, tp 2.2 ms, Ib 60 A). You raise the frequency to 150 Hz and change nothing else. What happens to the drops?
Mean current rises to 172 A, so the wire melts faster, but only 1.33 times, while pulses come 1.5 times as often. Drop volume = melting rate ÷ frequency falls, so the drop goes from 1.22 mm to 1.17 mm. Ip²tp is unchanged (352 A²s), so each pulse still detaches one drop.
Worked examples
Mean and rms current of a pulsed waveform · Ip 400 A for 2.2 ms, Ib 60 A for the rest of a 100 Hz period (T = 10 ms).
- Background time = 10 − 2.2 = 7.8 ms.
- Mean = (400 × 2.2 + 60 × 7.8) ÷ 10 = (880 + 468) ÷ 10 = 134.8 A.
- rms = √[(400² × 2.2 + 60² × 7.8) ÷ 10] = √38,008 = 195 A.
- Heat follows the mean power: at 24 V (assumed) the mean is 3.24 kW. Resistive heating of the stick-out follows rms², so rms matters for melting, mean for arc heat.
Answer: Mean 134.8 A, rms 195 A.
Does it detach one drop per pulse, and how big is the drop? · The same waveform, 1.2 mm wire. D = 236 × 1.2² = 339.8 A²s; window up to 1.51 D (borrowed from aluminium); melting rate MR = 0.478 Im + β Irms² with β fitted to the kernel point 9.5 m/min at 260 A.
- Ip² tp = 400² × 0.0022 = 352 A²s, between 340 and 513: one drop per pulse.
- β = (179.1 − 0.478 × 260) ÷ 260² = 8.12 × 10⁻⁴ mm³ per A²s.
- MR = 0.478 × 134.8 + 8.12 × 10⁻⁴ × 38,008 = 95.2 mm³/s, so wire feed = 95.2 ÷ 1.131 = 84.2 mm/s = 5.1 m/min.
- Drop volume = 95.2 ÷ 100 = 0.952 mm³, diameter = (6V/π)^(1/3) = 1.22 mm, 1.02 times the wire.
Answer: One drop per pulse of 1.22 mm at 5.1 m/min.
Too little peak energy · Same set-up but tp cut to 1.5 ms.
- Ip² tp = 400² × 0.0015 = 240 A²s, below D = 340.
- The pulse delivers 71 % of the energy needed, so a drop detaches only about every 1.4 pulses: drops lag behind and grow larger than the wire.
- The interactive marks this 'too little energy'. Fix it with a longer tp (2.2 ms) or a higher peak (above 476 A at 1.5 ms).
Answer: Ip²tp = 240 A²s is below the 340 A²s threshold: no clean one-drop-per-pulse transfer.
Plasma arc, electroslag, electrogas and atomic hydrogen welding
Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302045-A Unit 5 (electrogas, electroslag, atomic hydrogen, plasma arc and plasma transferred arc welding)MU not in syllabusKTU PEMET416 Module 3 (plasma arc welding: transferred and non-transferred arc); MET372 Module 5
What is plasma arc welding, and what is the keyhole mode?
Plasma arc welding squeezes a TIG-like arc through a small copper nozzle, so the plasma is narrow, stiff and hot. In the transferred arc the current flows from the electrode to the work; in the non-transferred arc it stays inside the torch between electrode and nozzle (used for spraying and for thin or non-conducting work). Above about 100 A the force of the plasma punches a hole through the plate and the pool closes behind it: the keyhole. TWI gives up to 10 mm in one pass, 6 mm as usual, with argon as plasma gas and argon plus 2 to 5 % hydrogen as shield.
How does electroslag welding work, and how fast does it climb?
Two plate edges stand upright with a gap between them, closed by water-cooled copper shoes. A bath of molten slag sits in the gap. The wire dips into it and the current heats the slag by its own resistance: there is no arc. The wire and the plate edges melt and the weld rises. In the book's 80 mm plate (assumed), a 30 mm gap and two wires at 450 A and 44 V deposit 23 kg/h and the weld climbs 20 mm/min. Here ṁ is the deposit mass rate, g the gap and t the thickness.
What does electroslag welding cost in heat, and what is the remedy?
All that power goes into one slow pass. The same case puts in 39.6 kW at 20 mm/min, 119 kJ per mm, against 2.3 kJ/mm for the book's SAW pass: 52 times more. The metal stays hot for a long time, so the grains in the weld and the heat-affected zone grow coarse and the toughness falls. The usual remedy is normalising the whole fabrication, which is often impractical. The time it saves is real: 50 min a metre against 2.4 h by multipass SAW, 2.9 times faster, ignoring set-up. Thickness guide: one wire per 25 to 75 mm.
How is electrogas welding different from electroslag?
Electrogas welding also climbs a vertical joint between copper shoes, but it keeps an arc burning. Shielding comes from a gas or from a flux-cored wire. It uses DC with the electrode positive, 100 to 800 A and 30 to 50 V. One electrode handles roughly 10 to 20 mm of plate; more wires take more. The joint must stay within 15° of vertical. It is used for ship hull plates and storage tanks. The heat input is lower than electroslag, so the coarse-grain problem is smaller, but the arc and the open gas shield need calm air.
What is atomic hydrogen welding?
An arc burns between two tungsten electrodes in a stream of hydrogen. In the arc the H2 splits into atoms, which takes 436 kJ per mole of H2 (twice the 218 kJ/mol enthalpy of the H atom, NIST). When the gas strikes the cold work the atoms recombine and give that energy back as heat, reaching 3,400 to 4,000 °C. Hydrogen also shields the weld, so no flux is needed. The work is not in the circuit. It is now largely replaced by GMAW and GTAW because inert gases got cheap.
On the same 80 mm joint you change from one wire to two wires, same current per wire, voltage and gap. What happens to the heat input per millimetre of weld rise?
Two wires double the power (19.8 to 39.6 kW) and also double the deposit, so the weld climbs twice as fast (10 to 20 mm/min). Heat per millimetre = power ÷ speed stays 119 kJ/mm. What changes heat input is the gap (a 36 mm gap gives 143 kJ/mm) or the volts and current per unit of deposit.
Worked examples
Rise speed and time for 1 m · THE STEEL as an 80 mm plate (assumed), gap 30 mm, two wires at 450 A, slag bath 44 V. Each wire deposits 0.0251 kg/h per ampere (from Ricci and Eagar's measured speeds: 0.954 m/h average, 28.5 mm gap, 50 mm plate, 425 A).
- Deposit = 2 × 0.0251 × 450 = 22.6 kg/h = 800 mm³/s.
- Rise speed = volume rate ÷ (gap × thickness) = 800 ÷ (30 × 80) = 0.333 mm/s = 20 mm/min.
- Time for 1 m = 1,000 ÷ 0.333 = 3,001 s = 50 min.
- Power = 44 × 900 = 39.6 kW. Heat input = 39.6 ÷ 0.333 = 119 kJ/mm.
Answer: 20 mm/min, 50 min per metre, 119 kJ/mm.
Electroslag against multipass SAW · Same plate, joined instead by multipass SAW in a double-V groove (60°, gap 2, face 2, cap 2) with the book's 4 mm wire at 600 A.
- Groove fill = 2 × 80 + 2 × 39² × tan 30° = 1,916 mm²; with both caps 2,050 mm², 16.09 kg per metre.
- SAW deposition 6.58 kg/h (the fit to Lincoln's data), so arc time = 16.09 ÷ 6.58 = 2.45 h per metre.
- Each pass is about 28 mm², so 2,050 ÷ 28 = 73 passes.
- ESW takes 0.83 h, in one pass: 2.9 times faster. Heat input per mm is 52 times higher (119 against 2.3 kJ/mm).
Answer: SAW needs 73 passes and 2.4 h per metre; ESW 50 min, with 52 times the heat per mm.
How many wires, and what is the minimum heat? · Two questions. (a) How many wires for a 150 mm plate, gap 30 mm, 450 A per wire, 44 V? Rule of thumb: one wire per 25 to 75 mm of thickness. (b) In the 80 mm case above, what share of the heat melts the deposit? Energy to melt steel Um = 10.5 J/mm³ (Manufacturing Processes book).
- (a) Wires = 150 ÷ 75 = 2 at the least; with 3 wires the rise is 16 mm/min.
- (b) Energy to melt the deposit alone = Um × gap × thickness = 10.5 × 30 × 80 ÷ 1000 = 25.1 kJ per mm of rise, in the 80 mm plate.
- The actual 119 kJ/mm is 4.7 times the melting energy: only 21 % melts the filler, the rest melts plate edges, heats the plate and the shoes.
Answer: At least 2 wires; about 21 % of the heat melts the deposit, the rest melts the plate edges and heats the plate and shoes.
Resistance welding processes: seam, projection, flash, upset, percussion and high-frequency
Which syllabus covers thisAU not in syllabusVTU BME302 Module 5 (resistance welding processes)SPPU not in syllabusMU not in syllabusKTU not in syllabus
How do seam, roll-spot and projection welding differ from spot welding?
All of them are resistance welding: current crosses the joint, the contact makes heat, and force squeezes the weld. Spot welding uses two pointed electrodes. Seam welding swaps them for rotating wheels and lays a row of nuggets. Overlapping nuggets make a leak-tight seam, as in tanks and drums. Spaced nuggets make a roll-spot weld. Projection welding puts small bumps on one part so the current and force land only there: a nut with 3 projections under 6 kN puts 2 kN on each bump (assumed).
How do you set the nugget pitch and overlap of a seam weld?
Take the book's 1.0 mm sheet (assumed): nugget D = 5√t = 5 mm. Mains is 50 Hz, so one cycle is 20 ms. At 1.5 m/min with 3 cycles on and 2 off, the pitch is v × 0.1 s = 2.5 mm. That is 50 % overlap and 400 welds a metre. At 5 m/min the pitch jumps to 8.33 mm: a string of spots, not a seam. Secondary sources ask for at least 15 % overlap for a gas-tight seam, so this setting tops out at 2.55 m/min. A leak test has the last word.
What are flash butt, upset and percussion welding?
In flash butt welding the two ends are clamped a little apart and voltage is applied. Tiny contacts arc and throw off sparks, the ends heat evenly, and a forging blow joins them. The molten metal is squeezed out as flash and trimmed. Machines often flash for a set distance, say 5 mm, before the upset starts. Rails, chain links and wheel rims are made this way. Upset butt welding presses the ends together first and heats them by contact resistance without arcing: it suits small bars and wire. Percussion welding fires a capacitor discharge arc and hits the parts together at once.
How do high-frequency resistance and induction welding make pipe, and what is skin depth?
A strip is rolled into a tube and the open seam is fed with current at about 400 kHz (assumed). At that frequency current crowds into a thin skin of depth δ. In cold steel (μr 100, assumed) δ is 30 µm; in copper it is 103 µm. The surface resistance ρ/δ of steel is 29 times copper's, so the steel edges heat while the copper contacts stay cool. The proximity effect pulls the current to the two facing edges. Squeeze rolls then forge them together.
How do you choose between these processes for a part?
Match the process to the geometry. Lap joints in sheet go to spot or seam welding. A tank that must hold pressure needs a seam: at 2.5 mm pitch the book's seam has 400 nuggets a metre, 12 times a spot row at an assumed 30 mm pitch. A part with a hard-to-reach joint or a nut to fix needs projections. Solid bars, rails and chain links need flash or upset welding, and thin-wall pipe in long lengths needs high-frequency welding. All of them need a clean, conductive surface and a joint that fits.
The 1.0 mm seam at 1.5 m/min (3 cycles on, 2 off) has 50 % overlap. You double the wheel speed to 3 m/min and change nothing else. What happens?
Pitch = v × (on + off) × 20 ms = 50 mm/s × 0.1 s = 5 mm. Nugget size comes from the sheet thickness, 5 mm, so the nuggets only touch: overlap = 1 − 5/5 = 0 %. Doubling the speed doubles the pitch. To hold the overlap at 3 m/min you must shorten the period: 1 cycle on and 1 off gives a pitch of 2 mm and 60 % overlap.
Worked examples
Seam pitch and overlap for a fuel-tank half (original case, assumed) · 0.9 mm steel sheet. Wheel speed 2.0 m/min. 50 Hz mains. The seam needs at least 25 % overlap. Choose the whole number of cycles for one on-off period.
- D = 5√0.9 = 4.74 mm.
- Wheel speed v = 2.0 m/min = 33.33 mm/s.
- Overlap ≥ 25 % needs pitch ≤ 0.75 × 4.74 = 3.56 mm.
- Period ≤ pitch / v = 3.56 / 33.33 = 107 ms = 5.34 cycles of 20 ms, so use 5 cycles in all (3 on, 2 off).
- Pitch = 33.33 × 0.1 s = 3.33 mm. Overlap = 1 − 3.33/4.74 = 29.7 %. Six cycles would give 4 mm and 15.7 %, only just above 15 %.
Answer: 5 cycles per nugget: pitch 3.33 mm, overlap 30 %, 300 nuggets per metre.
Fastest leak-tight wheel speed for the book's seam · 1.0 mm sheet, 3 cycles on and 2 off at 50 Hz, minimum overlap 15 % (typical, secondary sources).
- D = 5 mm. Largest pitch = (1 − 0.15) × 5 = 4.25 mm.
- One period is 5 cycles × 20 ms = 0.1 s.
- v = 4.25 mm / 0.1 s = 42.5 mm/s = 2.55 m/min.
- At 5 m/min the pitch is 8.33 mm, longer than the 5 mm nugget: there is no overlap, and a 3.33 mm gap is left between nuggets.
Answer: About 2.55 m/min. Above that, shorten the cycle count or accept a roll-spot weld.
Why a high-frequency pipe mill heats steel but not its copper contacts (assumed values) · 400 kHz. Cold steel: ρ 1.43e-7 Ω·m, μr 100. Copper: ρ 1.68e-8 Ω·m, μr 1. Compare the skin depth and the surface resistance ρ/δ.
- δ = √(2ρ/(ωμ)), ω = 2π × 4,00,000 = 2.513e6 rad/s, μ = μr × 4π × 10⁻⁷.
- Steel: δ = 30.1 µm. Copper: δ = 103.1 µm.
- Surface resistance: steel 4.75 mΩ per square; copper 0.163 mΩ per square.
- Ratio = 29.2. For the same current in the skin the steel edge makes about 29 times the heat.
Answer: δ about 30 µm in steel and 103 µm in copper; steel heats 29 times harder per unit of skin current.
Friction welding and friction stir welding: heat generation, tools and metal flow
Which syllabus covers thisAU not in syllabusVTU BME302 Module 5 (friction stir welding)SPPU 302045-A Unit 4 (friction stir welding)MU not in syllabusKTU PEMET416 Module 2 (friction and friction stir welding: process parameters, tools, metal flow); MET372 Module 3
How does friction welding work, and what are rotary and inertia welding?
One part spins while the other is held and pushed against it. Rubbing heats the faces. There are three phases: friction, where the faces heat; burn-off, where softened metal is squeezed out as flash and the parts shorten; and upset, where rotation stops and a forging force joins them. Rotary machines keep a motor driving throughout. Inertia machines spin a flywheel, disconnect it, and let ½Iω² turn into heat. An assumed flywheel of 1.5 kg·m² at 1,200 rpm stores 11.8 kJ: at most 24 J per mm² on a 25 mm bar, before losses.
How does friction stir welding join two plates without melting them?
A non-consumable tool with a shoulder and a pin spins and is plunged into the joint line, then travels along it. Friction and stirring soften the metal. It does not melt: the book's model puts the process at 750 K, 477 °C, which is 88 % of the 856 K solidus used for 6061. The pin carries softened metal round to the back, where the shoulder forges it. With no liquid there is no solidification cracking and no gas porosity from the pool, and distortion is low. Rail coaches, ship panels and battery trays are typical uses.
Where does the heat of FSW come from, and how do you size it?
Take the book's 6 mm 6061 plate (assumed), shoulder radius 9 mm, pin radius 3 mm, 800 rpm, 8 kN, 300 mm/min. Contact pressure is 35.4 MPa. With sliding friction (µ 0.4, assumed) the shear stress is 14.1 MPa and the heat is 2.19 kW: shoulder 1,743 W (80 %), pin side 382 W, pin tip 67 W. That is 438 J per mm of weld. If the surface sticks, τ = σy/√3 = 45.9 MPa and the heat is 7.1 kW.
What do the shoulder, pin and tilt of an FSW tool do?
The shoulder makes most of the heat here (80 %), forges the stirred metal and keeps it from squirting out. The pin stirs, and a thread on it drags metal down and round. Its length is just under the plate thickness: 5.7 mm for 6 mm (assumed 0.95 t), so the pin does not touch the backing bar. The tool is usually tilted a little so the shoulder's rear edge digs in and forges. On the advancing side the tool surface moves with the travel; on the retreating side it moves against it. The two sides flow differently, so a weld is checked on both.
What goes wrong in FSW, and how do you trade hot against cold?
The key ratio is turns per mm of weld. At 800 rpm and 300 mm/min the tool makes 2.67 turns per mm, or advances 0.375 mm a turn. Too cold (low rpm, high speed): the metal cannot flow, leaving a tunnel void or a kissing bond, a joint line closed but not bonded. Too hot: the plate softens, flash forms and the heat-affected zone loses strength. In the sliding model doubling rpm doubles the heat, 2.19 to 4.38 kW. Halving the speed doubles the joules per mm. The band on the page, 0.05 to 0.4 mm a turn, is typical and assumed, not sourced.
In the book's sliding model, you double the rotation speed from 800 to 1,600 rpm and keep force and travel speed. What does the heat per mm of weld do?
In the model every term is proportional to ω (shear stress τ = µp does not depend on speed), so Q doubles from 2.19 to 4.38 kW and J/mm doubles from 438 to 877. Real welds need not follow this: Wang et al. (2021) argue that heat depends on the stick-slip ratio of the interface more than on rotation speed alone. The model is a first estimate, not a promise.
Worked examples
Heat of the book's FSW weld (assumed case) · 6 mm 6061 plate. Shoulder radius 9 mm, pin radius 3 mm, pin length 0.95 t. 800 rpm, axial force 8 kN, travel 300 mm/min. Sliding friction, µ = 0.4.
- ω = 2π × 800/60 = 83.8 rad/s. Pin length H = 0.95 × 6 = 5.7 mm. Travel speed = 5 mm/s.
- Pressure p = F/(π(Rs² − Rp²)) = 8000/(π × (81 − 9)) = 35.37 MPa. τ = 0.4 × 35.37 = 14.15 MPa.
- Shoulder: (2/3)π ω τ (Rs³ − Rp³) = 1,743 W. Pin side: 2π ω τ Rp² H = 382 W. Pin tip: (2/3)π ω τ Rp³ = 67 W.
- Total Q = 2,192 W = 2.19 kW. Shoulder share = 79.5 %.
- Heat per mm = Q/v = 2,192/5 = 438 J/mm. Turns per mm = (800/60)/5 = 2.67.
Answer: 2.19 kW, 438 J/mm, 80 % from the shoulder.
Sliding or sticking: how much does the contact condition matter? · Same tool and settings. Sticking: τ = σy/√3 with the Johnson-Cook flow stress of 6061-T6 at 750 K, σy = 324 × (1 − ((750 − 297)/(856 − 297))^1.34), strain term dropped (assumed).
- σy = 324 × (1 − 0.8103^1.34) = 79.6 MPa. τ = σy/√3 = 45.9 MPa.
- Q scales with τ: 45.93/14.15 = 3.25.
- Q(sticking) = 2,192 × 3.25 = 7,115 W = 7.1 kW.
- Heat per mm = 1,423 J/mm.
Answer: 7.1 kW, about 3.2 times the sliding value. The truth lies between: a real tool both slides and sticks.
Energy of an inertia friction weld (assumed machine) · Flywheel of 1.5 kg·m² spun to 1,200 rpm, then released. Bar diameter 25 mm. Ignore losses (an upper bound).
- ω = 2π × 1200/60 = 125.7 rad/s.
- E = ½Iω² = 0.5 × 1.5 × 125.7² = 11,844 J.
- Area = π/4 × 25² = 491 mm².
- E/A = 24.1 J/mm².
Answer: 11.8 kJ, at most 24 J per mm² of interface.
Explosive, diffusion, cold pressure, ultrasonic, forge and roll welding
Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302045-A Unit 4 (cold pressure welding, diffusion bonding, explosive, ultrasonic, forge, roll and hot pressure welding)MU not in syllabusKTU PEMET416 Modules 1-2 (diffusion, cold pressure, explosive and ultrasonic welding); MET372 Modules 2-4
How does explosive welding join two plates?
The flyer plate sits above the base plate with a small gap, and a layer of explosive lies on top. Detonation starts at one end and runs along at speed Vd. The blast drives the flyer down at speed Vp, so it hits the base at a small angle β and the collision point runs along at Vd. At that point the plate surfaces act like fluids: oxide films and a thin layer of metal are blown out ahead as a jet, and clean metal meets under huge pressure. The interface is wavy. Take a 6 mm steel flyer (assumed) with Vd = 2,500 m/s: Vp is 393 m/s and β = 9°.
How do you find the flyer speed and the weldability window?
The Gurney equation gives Vp from the load ratio R = C/M, explosive mass over flyer mass per area. For a welding explosive √(2E) is about Vd/3 (assumed). The book's case: R = 0.8, √(2E) = 833 m/s, Vp = 393 m/s, β = 2·asin(Vp/2Vd) = 9°. The window (Grignon et al. 2004) has a lower limit, 6° here, an upper limit and a sonic limit: Vd must stay below the plate's sound speed, 4,497 m/s for steel. Inside all three the weld is good; outside, the jet fails or the joint melts.
What are diffusion welding and cold pressure welding?
Diffusion welding presses two clean surfaces together at 50 to 75 % of the absolute melting temperature, in a vacuum or inert gas, for minutes to hours. Atoms cross the interface and the voids close. For 6061, with the 856 K solidus, that is 428 to 642 K, or 155 to 369 °C. There is little visible deformation, so it joins titanium, dissimilar metals and foil stacks. Cold pressure welding needs no heat: heavy deformation of soft, clean metals such as aluminium and copper breaks the surface films and brings fresh metal into contact.
How does ultrasonic welding work, and why is the horn the size it is?
A transducer vibrates a horn at 15 to 40 kHz. The horn presses on the stack and moves it sideways along the joint, parallel to the faces. The shearing action breaks the oxide and bonds the metals without melting. It suits foils, wires, thin sheets and battery tabs. The horn is tuned to half a wavelength. For an aluminium rod (assumed), wave speed √(E/ρ) = 5,055 m/s, so the half wavelength is 126 mm at 20 kHz and 63 mm at 40 kHz.
What are forge, roll and hot pressure welding?
Forge welding is the blacksmith's weld: heat both pieces to a white heat, add flux, and hammer them together. Hot pressure welding does the same with a press. Roll welding passes a stack through rolls. The squeeze thins the stack, which spreads the surfaces and breaks the films so the layers bond. A pair of 6 mm plates rolled to 8 mm total is a 33 % reduction (assumed). Clad plate, coinage blanks and bimetal strip are made this way. All three need clean, oxide-free faces and enough deformation.
A 6 mm steel flyer is welded to steel with R = 0.8. An operator switches to an explosive that detonates at 4,800 m/s instead of 2,500 m/s. Which limit is the problem?
Vp scales with Vd (√2E = Vd/3), so β stays at 9° and sits above the lower limit, which falls to 3.1°. But the collision point moves at Vd = 4,800 m/s, above the steel's bulk sound speed of 4,497 m/s. Supersonic collision gives a shock, not a jet, and the plates do not weld cleanly.
Worked examples
Flyer speed and dynamic angle by hand (assumed explosive) · Detonation velocity 2,500 m/s, √(2E) = Vd/3. Load ratio R = C/M = 1 (explosive mass equals flyer mass per area).
- √(2E) = 2500/3 = 833.3 m/s.
- Bracket = ((1 + 2/R)³ + 1)/(6(1 + 1/R)) + 1/R = (27 + 1)/12 + 1 = 3.333.
- Vp = 833.3 / √3.333 = 456.4 m/s.
- β = 2·asin(Vp/(2Vd)) = 2·asin(456.4/5000) = 10.48°.
Answer: Vp = 456 m/s and β = 10.5°.
Smallest explosive load that still welds steel to steel (assumed) · 6 mm steel flyer on steel, Vd = 2,500 m/s, clean surfaces (k1 = 0.6), steel 150 HV (H = 1.471 GPa), density 7,850 kg/m³, explosive density 800 kg/m³.
- Lower limit β = 0.6 √(H/(ρVw²)) = 0.6 × √(1.471e9/(7850 × 2500²)) = 0.1039 rad = 5.95°.
- Needed Vp = 2Vd·sin(β/2) = 5000 × sin(2.98°) = 259.6 m/s.
- Solve Gurney for R: R = 0.459 (bisection).
- Flyer mass M = 7850 × 0.006 = 47.1 kg/m². C = 0.459 × 47.1 = 21.6 kg/m², a layer 27 mm thick.
Answer: R must be at least 0.46: about 22 kg of explosive per m², a 27 mm layer.
Aluminium flyer on steel: is the set-up inside the window? (assumed) · 3 mm Al 6061-O flyer (38 kgf/mm², 2,700 kg/m³, E 69 GPa, ν 0.33) on a steel base. Vd = 2,200 m/s, R = 1.2, clean surfaces.
- M = 2700 × 0.003 = 8.1 kg/m². C = 1.2 × 8.1 = 9.72 kg/m², a layer 12.1 mm thick.
- √(2E) = 2200/3 = 733.3 m/s. Vp = 450.6 m/s. β = 11.76°.
- Lower limit for the pair, (Ha + Hb)/(ρa + ρb): 6.53°. Upper limit: the equation gives a sine above 1, so there is no practical upper limit for 3 mm.
- Sound speeds: Al 5,005, steel 4,497 m/s. The slower plate sets the limit, 4,497 m/s. Vd = 2,200 is well below it.
Answer: β = 11.8° is above the lower limit (6.5°) and Vd is subsonic: inside the window.
Adhesive bonding: adhesives, joint design and the stress in a lap joint
Which syllabus covers thisAU not in syllabusVTU BME302 Module 5 (adhesive bonding)SPPU 302045-A Unit 4 (advances in adhesive bonding)MU not in syllabusKTU PEMET416 Module 1 (adhesive bonding: adhesives, bonding methods); MET372 Module 2
What kinds of structural adhesive are there, and how stiff are they?
Epoxies are two-part (resin and hardener) or heat-cured and give strong, durable bonds. Acrylics cure fast and tolerate oily surfaces. Cyanoacrylates (super glue) set in seconds on small, tight-fitting parts but are brittle. Polyurethanes stay flexible, which suits vibration and mixed materials. Hot melts are thermoplastics that grip as they cool. An epoxy's shear modulus of about 0.83 GPa (assumed, as in the Delft toolbox example) is 31 times softer than aluminium's 26 GPa. That softness is what lets the load spread, and also what decides where it peaks.
Why do surface preparation and curing decide the joint?
A bond is only as good as its weakest layer. Grease, oxide and moisture on the metal make the failure run along the interface, called adhesion failure, at a fraction of the adhesive's strength. So degrease, abrade or etch, and prime or anodise aluminium, and bond soon after. A good test pull tears through the adhesive layer: cohesive failure. Curing needs the right mix ratio, time and temperature. Heat speeds a cure and can raise strength, but a cure that is too hot or too quick leaves stress and voids. Keep a thin, even bond line of about 0.1 to 0.3 mm.
Why do the ends of a bonded lap joint carry the load?
Take two 2 mm aluminium strips and 0.2 mm of epoxy (assumed), 20 mm overlap, 100 N/mm. Average shear is 100/20 = 5 MPa. But the strips stretch, so the load transfers near the ends. Volkersen's shear-lag solution gives a peak of 12.4 MPa, 2.49 times the average, and almost nothing in the middle (2.1 MPa). Overlap beyond about 15 mm only adds unused glue. Doubling it to 40 mm lowers the peak by only 1.5 %. The model ignores bending: real peaks are higher.
Which joint designs work, and why is a butt joint weak?
Adhesives like shear and compression and dislike peel and cleavage, which pull the layer apart at one edge. A lap joint puts the glue in shear but its end load bends the strips, adding peel. A scarf joint cuts both ends at a shallow angle: at 10° the 2 mm strips give a uniform 8.6 MPa shear and 1.5 MPa tension over 12 mm. A strap joint adds a plate across a butt. A plain butt joint has only the strip's own thickness to bond: 100 N/mm over 2 mm is 50 MPa straight tension, with any misalignment adding peel. It is the weakest layout.
When should you bond, weld or rivet?
Bonding spreads the load over the whole area, adds no heat-affected zone and joins dissimilar materials such as aluminium to steel or to composites without galvanic or thermal trouble. It also seals the joint. The limits: most structural adhesives lose strength at high temperature, ageing and moisture attack the interface, peel is weak, a bond is hard to inspect and cannot be taken apart. Welding wins at high temperature and thick sections; rivets give a visible, mechanical back-up. Combined methods, such as rivet-bonding and weld-bonding, use the adhesive for sealing and fatigue and the fasteners for peel.
A 20 mm lap of two 2 mm aluminium strips with 0.2 mm epoxy carries 100 N/mm and peaks at 12.4 MPa at the ends. Which change lowers that peak the most?
Doubling the overlap only brings the peak to 12.3 MPa (1.5 % lower): the middle carries almost nothing. Thicker adherends are stiffer, so they share load more evenly: 9.2 MPa, 26 % lower. A thinner bond line or a stiffer adhesive both raise λ and concentrate the load: 17.4 and 17.4 MPa.
Worked examples
Shear stress in the book's bonded lap joint (assumed) · Two 2 mm aluminium strips (E = 69 GPa), epoxy 0.2 mm thick with G = 830 MPa, overlap 20 mm, load 100 N per mm of width.
- λ² = (G/η)(1/(E1t1) + 1/(E2t2)) = (830/0.2)(2/(69000 × 2)) = 0.0601 mm⁻², so λ = 0.2452 per mm.
- Average τ = P/l = 100/20 = 5 MPa. λl/2 = 2.452.
- Peak τ = (Pλ/2)·coth(λl/2) = 12.262 × 1.0149 = 12.45 MPa. Ratio = 2.49.
- Middle of the overlap: (Pλ/2)/sinh(λl/2) = 2.13 MPa.
- Check: the area under τ(x) over 20 mm is 100 N/mm, equal to the load.
Answer: Average 5 MPa, peak 12.4 MPa at each end (2.5 times the average).
Does a longer overlap help? (same joint) · As above, but the overlap is doubled to 40 mm at the same 100 N/mm. Then find the load per width the 40 mm joint carries at the old peak stress.
- λ is unchanged (0.2452/mm). λl/2 = 4.9, so coth is 1.0000.
- Peak = Pλ/2 = 12.26 MPa, against 12.45 for 20 mm: 1.5 % lower.
- Average falls to 100/40 = 2.5 MPa, but the ends see nearly the same stress.
- Load at the old peak: 100 × 12.45/12.26 = 101.5 N/mm.
- The useful length (peak within 5 % of its limit) is 2·atanh(1/1.05)/λ = 15.1 mm.
Answer: Capacity rises only from 100 to 101.5 N/mm for twice the glue. Past about 15 mm, thicker or stiffer strips help more than overlap.
Scarf joint against lap joint at the same load (original case, assumed) · The same 2 mm strips and 100 N/mm, joined by a scarf cut at 10° to the load axis.
- Strip stress = 100/2 = 50 MPa. Bond-line length = t/sin 10° = 11.5 mm.
- Shear τ = σ sinθ cosθ = 50 × 0.1736 × 0.9848 = 8.55 MPa (uniform).
- Normal σn = σ sin²θ = 1.51 MPa.
- Lap joint of 20 mm: average 5 MPa but peak 12.4 MPa.
Answer: The scarf carries the same load at a uniform 8.6 MPa, against a 12.4 MPa peak for the lap, but needs a precisely cut joint.
Electron beam welding: the gun, vacuum, beam power and deep narrow welds
Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302045-A Unit 5 (electron beam welding)MU not in syllabusKTU PEMET416 Module 3 (electron beam welding); MET372 Module 1
How does an electron beam gun make and aim a beam?
A hot cathode gives off electrons. A high voltage between cathode and anode, 30 to 150 kV, speeds them up. At 60 kV an electron reaches 0.446 of the speed of light, because its energy is a fair share of its rest energy of 511 keV. Magnetic coils then focus the beam, as a lens focuses light, and deflection coils steer it. Beam power is just voltage times current: 60 kV at 100 mA is 6 kW. The gun must sit in high vacuum, or the hot cathode burns out.
What do the voltage, current and vacuum do to the beam?
Voltage sets the electron speed. Current sets the power. The spot size sets the power density: 6 kW into a 0.3 mm spot is 85 kW/mm², far above the 0.001 to 1 MW/cm² window of arc welding. The vacuum sets how far the beam survives. Gas molecules scatter electrons: at 1 atm a gas molecule travels only 66 nm between collisions, at 10⁻⁵ mbar it travels 6.7 m. That is a pessimistic scatter length, since fast electrons collide far less often than molecules do. The interactive lets you try all three.
Why is an electron beam weld deep and narrow if electrons only reach a few microns?
A 60 kV electron stops within about 10 µm of the iron surface (Kanaya-Okayama range). The beam does not drill by penetration. It dumps 85 kW/mm² into a thin skin, vaporises metal and digs a keyhole: a tube of vapour held open by its own pressure, with molten metal flowing around it. The beam follows the keyhole down. Typical depth to width ratios are 50:1 in high vacuum, 20:1 in medium vacuum and 5:1 with no vacuum (Open University table); an arc weld is usually wider than it is deep.
What are the vacuum levels, and what does each cost you?
High vacuum (10⁻⁴ to 0.1 Pa) gives the deepest and narrowest weld, 50:1 and up to 150 mm of steel, but the part must go into a chamber and pump-down takes time. Medium vacuum (0.1 to 3,000 Pa) pumps faster and welds to about 50 mm at 20:1. Non-vacuum EBW fires the beam into air through pumped stages: no chamber, but only about 25 mm at 5:1, because air scatters the beam. Zinc, cadmium and magnesium vaporise too easily to weld in vacuum.
What are the limits of EBW, and where is it used?
The part must fit tightly, because a beam 0.3 mm wide cannot bridge a gap, and the seam must be on the beam's line of sight. Chambers and pumps are expensive. Electrons hitting metal make X-rays, so the chamber is shielded with steel or lead. In exchange you get almost no distortion and a very narrow HAZ. That is why it welds gears, turbine and aero-engine parts, nuclear components and thick pressure vessels. Keyence quotes steel from 0.1 to 200 mm.
You double the accelerating voltage from 60 to 120 kV at the same beam current and spot. What happens to the power density?
Power = voltage × current, so the power doubles from 6 to 12 kW. The spot is unchanged, so the power density doubles to 170 kW/mm². The electrons also run faster, 0.446 c to 0.587 c, not twice as fast: relativity caps the speed at c.
Worked examples
Electron speed and beam power · A gun runs at 60 kV and 100 mA. Rest energy of an electron = 511 keV.
- γ = 1 + eV/(mc²) = 1 + 60/511 = 1.1174.
- v/c = √(1 − 1/γ²) = √(1 − 1/1.2486) = 0.4462.
- v = 0.4462 × 2,99,792 km/s = 1,33,775 km/s.
- P = V I = 60 kV × 100 mA = 6,000 W = 6 kW.
Answer: 0.446 c, about 134 thousand km/s, and 6 kW.
Power density, and the current for the same power at 150 kV · The beam above (6 kW) is focused to a 0.3 mm spot.
- Spot area = π × 0.3²/4 = 0.0707 mm².
- Power density = 6 kW / 0.0707 mm² = 84.9 kW/mm² = 84,883 W/mm².
- That sits inside the 10⁴ to 10⁷ W/mm² range quoted for EBW.
- At 150 kV the same 6 kW needs only I = P/V = 6,000/1,50,000 = 0.04 A = 40 mA, and the electrons reach 0.634 c.
Answer: 85 kW/mm²; 40 mA at 150 kV.
Which vacuum can you use over 100 mm? · Gun-to-work distance 100 mm. Compare 10⁻⁵ mbar, 0.1 mbar and 1 atm (1,013 mbar), 20 °C, nitrogen molecules of 0.37 nm.
- Number density n = p/(kT); mean free path λ = 1/(√2 n π d²).
- At 10⁻⁵ mbar: λ = 6.65 m. At 0.1 mbar: λ = 0.67 mm. At 1 atm: λ = 66 nm.
- Chance a molecule-sized collision happens in 100 mm = 1 − exp(−L/λ): 1.5 % at 10⁻⁵ mbar, essentially 100 % at the other two.
- These are pessimistic: a fast electron has a much smaller collision cross-section than a molecule, which is why non-vacuum EBW works at all over a short 10 to 20 mm stand-off.
Answer: Only high vacuum passes 100 mm cleanly (λ = 6.7 m); medium vacuum and air need a much shorter stand-off.
Laser beam welding: laser types, focusing, absorption and keyhole welding
Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302045-A Unit 5 (laser beam welding)MU not in syllabusKTU PEMET416 Module 3 (laser beam welding: types of lasers, process parameters); MET372 Module 1
What laser types weld metal, and how does the beam get to the joint?
The CO₂ laser (10.6 µm) is a gas laser: its beam travels by mirrors, because glass fibre does not carry 10.6 µm. Nd:YAG (1.064 µm) and fibre lasers (1.07 µm) have a shorter wavelength that goes down an optical fibre to a robot-held head. Disk and diode lasers are the other families. The short wavelength matters twice: steel absorbs 36 % of 1 µm light on a cold surface but only about 3.5 % of 10.6 µm (model), and a shorter wavelength focuses to a smaller spot.
How small can a laser be focused, and how long does that focus last?
A raw beam of diameter D focused by a lens of focal length f gives a spot d₀ = 4λfM²/(πD). M² (1 for a perfect beam) says how far the beam is from ideal. A fibre laser (λ = 1.07 µm, D = 20 mm, f = 200 mm, M² = 10) gives 136 µm. The beam stays near that size over the Rayleigh length z_R = πw₀²/(λM²) = 1.36 mm on each side. The ratio f/D is the f-number, here 10. Short f-number: tiny spot but a very short focus to hold.
What is conduction mode, what is keyhole mode, and what power density separates them?
Below about 0.5 MW/cm² the laser only melts the surface: conduction mode, wide and shallow, a bit like an arc weld. Above it, the surface boils. The vapour pressure digs a keyhole, and the beam bounces down inside it, so almost all of the light is absorbed. OSTI report 10807 puts the start at over 0.5 MW/cm² and about 1 MW/cm² to hold the keyhole open. The 136 µm spot needs only 73 W to start one and 146 W to hold it.
Why do aluminium and copper weld worse with a laser than steel?
A cold, shiny metal reflects most of the beam. At 1 µm a measured 35.9 % of the light is absorbed by iron but only 4.8 % by aluminium, and the free-electron model gives about 4.6 % for copper. At 10.6 µm the model gives 3.5 % for iron, 1.9 % for aluminium and 1.5 % for copper. Once a keyhole forms the absorption jumps. So thick aluminium and copper need high power density to get started, and the start of a pass is the unstable moment.
What else controls a laser weld besides power and spot size?
Travel speed, the focus position (on the surface or a little below it), the shielding gas and the joint fit-up. A gap wider than the spot lets the beam fall through, and a spot of only 136 µm cannot bridge a gap. A plasma plume of ionised vapour can shield the beam, mostly with CO₂ lasers, and a side jet of helium or argon blows it away. Laser-arc hybrid welding adds an arc to bridge gaps and widen the weld. Tailored blanks and battery tabs are common jobs.
You swap the focusing lens for one with half the focal length, with everything else unchanged. What happens to the spot size and the Rayleigh length?
The spot is proportional to f, so it halves (136 to 68 µm). The Rayleigh length is proportional to w₀², so it falls to a quarter (1.36 to 0.34 mm). The irradiance goes up four times, but the focus is four times harder to hold.
Worked examples
Spot size, Rayleigh length and f-number · A fibre laser, λ = 1.07 µm, raw beam D = 20 mm, lens f = 200 mm, M² = 10.
- d₀ = 4λfM²/(πD) = 4 × 1.07×10⁻³ × 200 × 10 / (π × 20) = 0.1362 mm = 136 µm.
- w₀ = d₀/2 = 0.0681 mm.
- z_R = πw₀²/(λM²) = π × 0.0681² / (1.07×10⁻³ × 10) = 1.36 mm, so the depth of focus 2z_R = 2.72 mm.
- f-number = f/D = 200/20 = 10. Check: at z = z_R the radius is √2 w₀ = 0.0963 mm.
Answer: Spot 136 µm, Rayleigh length 1.36 mm, f/10.
Is it keyhole welding? · The 136 µm spot above carries 4 kW. The keyhole starts above 0.5 MW/cm² and is held at about 1 MW/cm².
- Spot area = π × (0.01362 cm)²/4 = 0.000146 cm².
- Irradiance = 4,000 W / 0.000146 cm² = 27.4 MW/cm².
- That is 55 times the start threshold: keyhole mode with plenty to spare.
- Power to just start a keyhole = 0.5×10⁶ × 0.000146 = 73 W; to hold it, 146 W.
Answer: 27.4 MW/cm²: keyhole. Even 73 W would start one.
CO₂ against fibre on steel · A CO₂ laser with D = 20 mm, f = 150 mm, M² = 1.1 against the fibre laser above. Iron resistivity 9.7×10⁻⁸ Ω·m.
- CO₂ spot = 4 × 10.6×10⁻³ × 150 × 1.1 / (π × 20) = 111 µm, about the same as the fibre's 136 µm, thanks to its excellent beam quality.
- Hagen-Rubens absorptivity A = 2√(2ε₀ωρ): at 10.6 µm, ω = 2πc/λ = 1.78×10¹⁴ rad/s, so A = 3.5 %.
- For the fibre laser on cold iron the measured value is 35.9 %: about 10 times more.
- The model fails for iron at 1 µm (it gives about 11 %, because it misses interband absorption), so the measured figure is used there.
Answer: Same spot size; steel absorbs about 10 times more of the fibre beam on a cold surface.
Brazing, soldering, MIAB, underwater welding and micro-joining
Which syllabus covers thisAU not in syllabusVTU BME302 Module 5 (soldering and brazing)SPPU 302045-A Unit 5 (underwater welding)MU not in syllabusKTU PEMET416 Module 4 (MIAB, underwater welding, brazing, micro- and nano-joining); MET372 Modules 4-5
What separates brazing and soldering from welding?
In welding the base metal melts. In brazing and soldering it does not: a filler with a lower melting point is drawn into a close gap by capillary action, wets the surfaces and freezes. AWS draws the line between the two at 450 °C (840 °F): a filler whose liquidus is above it brazes, below it solders. Brazing joints are stronger and run hotter; soldering suits electronics and plumbing. Neither needs a weld pool, so dissimilar metals, thin sections and parts that would distort are routine.
How fast does a filler run into a gap, and what gap works best?
Capillary pull between plates a gap g apart is Δp = 2γcosθ/g. For silver filler (γ = 0.9 N/m, assumed) in a 0.1 mm gap that is 17.4 kPa. The Washburn form L² = γ g cosθ t/(3η) then fills a 12 mm joint in 20 ms. Real brazes take seconds, because heating, flux and wetting are slower than the flow. Lucas-Milhaupt's ideal clearance for flux brazing with silver is 0.051 to 0.127 mm. Too tight starves the joint, too wide loses the pull.
How are brazed joints heated and protected?
Torch brazing is manual and fast, with a flux paste to dissolve oxide. Furnace brazing heats many parts at once in a controlled atmosphere or vacuum, so no flux is needed and tight clearances of 0 to 0.051 mm work. Induction brazing heats one spot in seconds. Dip brazing uses a molten salt bath, common for aluminium. Design the joint as a lap about three times the thickness of the thinner part, so that the filler's shear strength carries the load rather than the butt face.
What is magnetically impelled arc butt welding (MIAB)?
Two tube ends are held about 1 to 2 mm apart. An arc is struck across the gap and a radial magnetic field, made by a coil, pushes it round the ring. The force on an arc of length L is F = B·I·L: with B = 50 mT (assumed), I = 800 A and L = 2 mm that is 0.08 N. The spinning arc heats both ends evenly, then a forging blow joins them and squeezes the molten metal out. Runs on 3.5 to 5.5 mm tube used 900 to 1,100 A for 6 to 12 s. It is used on automotive tubes and axle parts.
How is welding done underwater, and what does depth do?
Wet welding uses a waterproofed electrode with the diver in the water: cheap, but the fast quench makes hard, hydrogen-rich welds. Dry hyperbaric welding puts the weld in a pressurised chamber, giving much better quality. Pressure rises by about 1 atm every 10 m: p = p₀ + ρgh. At 30 m of seawater (ρ = 1,025 kg/m³) the absolute pressure is 4.03 bar, 4 atm, which constricts the arc and raises its voltage. Micro-joining (wire bonding, sintered silver) is the opposite scale: micro-metre wires joined by ultrasonic energy or silver particles.
A silver braze fills a 0.10 mm gap. You machine the parts to a 0.05 mm gap. What happens to the capillary fill time and the pull?
Pull is 2γcosθ/g, so halving the gap doubles it (17.4 to 34.8 kPa). The fill time is 3ηL²/(γ g cosθ), so it also doubles (19.9 to 39.8 ms): the narrower channel pulls harder but resists the flow more. At 0.05 mm you are also below the 0.051 mm edge of the flux-brazing band, where the flux cannot flow out.
Worked examples
Washburn fill time and capillary pull · Silver filler (assumed γ = 0.9 N/m, η = 4 mPa·s, ρ = 9,000 kg/m³, contact angle 15°) in a 0.10 mm gap, 12 mm long.
- Pull Δp = 2γcosθ/g = 2 × 0.9 × cos 15° / 0.0001 = 17,387 Pa = 17.4 kPa.
- Washburn: t = 3ηL²/(γ g cosθ) = 3 × 0.004 × 0.012² / (0.9 × 0.0001 × cos 15°) = 0.0199 s = 19.9 ms.
- Check by marching the flow velocity ū = g²Δp/(12ηL) in small steps: the same 19.9 ms to within 1 %.
- This is a lower bound: the shop time is set by heating and flux, not by viscosity.
Answer: 17.4 kPa and about 20 ms.
How high does the filler climb against gravity? · The same silver filler in a vertical 0.10 mm gap.
- Pull Δp = 17,387 Pa. A column of height h weighs ρgh = 9,000 × 9.81 × h per unit area.
- h = Δp/(ρg) = 17,387 / (9,000 × 9.81) = 0.197 m = 197 mm.
- Halve the gap to 0.05 mm and the rise doubles to 394 mm. In a 0.3 mm gap it is only 66 mm.
Answer: About 197 mm, more than any real joint is tall, so the fill is capillary-limited only in wide gaps.
MIAB arc force and the pressure at 30 m · MIAB: radial B = 50 mT (assumed), arc current 800 A, arc length 2 mm. Underwater: 30 m of seawater, ρ = 1,025 kg/m³.
- Force per mm of arc = B·I·1 mm = 0.05 × 800 × 0.001 = 0.04 N.
- Force on the 2 mm arc = 0.04 × 2 = 0.08 N, tangential to the tube.
- Pressure at 30 m = 1,01,325 + 1,025 × 9.807 × 30 = 4,02,879 Pa = 4.03 bar absolute.
- That is 3.98 atm, about 4 times the surface pressure.
Answer: 0.08 N on the arc; 4.03 bar absolute at 30 m.
Surfacing, cladding, hardfacing, thermal spraying and welding automation
Which syllabus covers thisAU not in syllabusVTU not in syllabusSPPU 302045-A Units 4-5 (cladding; robotic welding and welding automation)MU not in syllabusKTU not in syllabus
What are surfacing, cladding, hardfacing and buttering?
Surfacing is welding a layer on a surface for its properties, not to join. Cladding puts a corrosion-resistant layer, such as stainless or a nickel alloy, on a cheaper steel: a pressure vessel's inside, say. Hardfacing puts on a wear-resistant layer, such as cobalt-based Stellite or chromium carbide alloys, on a bucket tooth or a roll. Buttering is a transition layer of a compatible filler laid on one member before the joint is made, so a dissimilar weld is made between like metals.
What is dilution, and how much do the processes give?
Dilution is the share of a clad bead that is melted base metal: D = Am/(Ad + Am), where Ad is the deposit above the surface and Am the base melted below it. For Ad = 30 mm² and Am = 7.5 mm², D = 20 %. Typical ranges: laser powder 5 to 10 %, PTA 5 to 20 %, GMAW or GTAW up to 30 % (Lincoln Electric and surfacing papers). Wire SAW is about 30 % (typical, assumed). Less dilution means the first layer is already close to the filler's composition.
How many layers does a clad need, and how does overlap affect it?
Each new layer melts a fraction D of the layer below, so C_n = C_f + (C_b − C_f)Dⁿ. A 309L filler (24 % Cr) on the book's E350 plate (0.03 % Cr, assumed analysis) at D = 20 % gives 19.2 % Cr in layer 1, above an assumed target of 18 %. At D = 30 % layer 1 has 16.8 % and layer 2 has 21.8 %: two layers. Beads are laid side by side with about 50 % overlap, a common target: that leaves a ripple of 25 % of the bead height (parabolic beads, a model).
How does thermal spraying differ from cladding?
Thermal spraying melts or softens a powder or wire in a flame, an arc, a plasma or a high-velocity oxy-fuel (HVOF) jet and throws the droplets at a cold, roughened surface. The coating sticks mechanically, with little or no melting of the base metal: no dilution and almost no distortion, but some porosity and a bond weaker than a weld. A spray-and-fuse step can remelt a self-fluxing alloy into a true metallurgical bond. Spraying suits wear, heat and corrosion coatings on shafts and rolls, and it can coat ceramics a weld cannot.
What does welding automation add?
Mechanised welding moves the torch on a carriage or a column and boom; automatic welding adds sensors that adjust the weld; robots do both on a programmable arm. Seam tracking, by touch sensing, an arc sensor or a laser line, follows the joint when fit-up varies. A weave pattern fills a wide groove. A robot cell pairs the arm with a positioner and fixtures that locate the parts the same way every time, and it must have guarding and an emergency stop. Repeatable travel speed is the big gain: heat input stays on the WPS.
A 309L overlay (24 % Cr) on mild steel is welded with 40 % dilution. How many layers are needed to reach 18 % Cr?
Layer 1 = 24 − 23.97 × 0.4 = 14.4 % Cr. Layer 2 = 24 − 23.97 × 0.4² = 20.2 % Cr, above 18 %. Layers converge on the filler's 24 % because each dilutes the one below by only 40 %.
Worked examples
Dilution from bead areas · A GMAW bead on the book's E350 plate (assumed): deposit above the surface 30 mm², melted base 7.5 mm².
- D = Am/(Ad + Am) = 7.5/(30 + 7.5) = 0.2 = 20 %.
- Check against the usual GMAW range, up to 30 %: inside it.
- Bead of width 10 mm (assumed) as a parabola: height = 3Ad/(2w) = 4.5 mm, melt depth = 3Am/(2w) = 1.125 mm.
- To halve D to 10 % at the same deposit, Am = D Ad/(1 − D) = 3.33 mm².
Answer: 20 % dilution; Am must fall to 3.3 mm² for 10 %.
Chromium in the layers · 309L filler 24 % Cr (AWS A5.9 range 23 to 25 %) on the book's E350 plate (0.03 % Cr, assumed). Target at least 18 % Cr (assumed).
- D = 20 %: layer 1 = 24 + (0.03 − 24) × 0.2 = 19.206 % Cr. It meets 18 % in one layer.
- D = 30 %: layer 1 = 16.81 % (short), layer 2 = 24 − 23.97 × 0.09 = 21.84 %: two layers.
- The dilution that just reaches 18 % in layer 1 solves 24 − 23.97 D = 18: D = 25 %. Check: D = 25 % gives 18.01 %.
- That agrees with the guidance that dilution above about 25 % is not advisable for stainless overlays.
Answer: One layer at 20 %; two layers at 30 %; the limit for one layer is 25 %.
Bead overlap and layer thickness · Beads of width 10 mm and deposit area 30 mm² (assumed), parabolic, laid with 50 % overlap.
- Step between bead centres = w(1 − o) = 10 × 0.5 = 5 mm.
- Average layer thickness = deposit area / step = 30/5 = 6 mm.
- Ripple: the valley between beads is (s/w)² = (5/10)² = 0.25 of the bead height 4.5 mm, so 1.12 mm.
- At 80 % overlap the step is 2 mm, the layer 15 mm thick and the ripple only 0.18 mm, but each bead remelts more of the last.
Answer: 6 mm layer with 25 % ripple at 50 % overlap.
Heat flow in welding: Rosenthal's moving source, thick and thin plates, cooling time
Which syllabus covers thisAU CME395 Unit III (physical metallurgy of welding)VTU BME302 Module 5 (thermal effects in welding)SPPU 302045-A Unit 3 (weld thermal cycles and their effects)MU not in syllabusKTU not in syllabus
Why does the way heat flows decide how a weld turns out?
A weld is a moving heat source. The arc puts in q = k·U·I watts, the plate drains it away, and everything you care about follows: how big the pool is, how wide the heat-affected zone gets, how fast the metal cools and so what it turns into. The book's GMAW pass (assumed procedure: 28 V, 260 A, 6 mm/s, k = 0.8) puts in 5,824 W, which is 0.971 kJ/mm. In the book's E350 plate (assumed heat analysis) that makes a pool 8.6 mm wide and 27 mm long, and the centreline cools from 800 to 500 °C in about 5.1 s.
What is Rosenthal's solution, and what does it leave out?
Rosenthal (1941) solved the heat equation for a point source moving at steady speed over a thick plate. In the frame that travels with the arc the temperatures stop changing: you get fixed isotherms, long and thin at speed. It assumes constant properties, no latent heat, no stirring in the pool and no loss from the surface. So it is a first estimate. For steel the book uses effective values, k = 24.1 W/m·K and ρc = 7.83 J/cm³·K, picked so the model matches the EN 1011-2 cooling times. Cold steel is k = 51 W/m·K and ρc = 3.8: hot steel conducts less, and the effective ρc also carries the latent heat.
When is a plate 'thick' and when is it 'thin' for heat flow?
Thick means the heat spreads down as well as sideways (3-D, a point source). Thin means it goes through the plate at once and then spreads only sideways (2-D, a line source). The dividing line is the transition thickness, which grows with heat input. EN 1011-2 gives d_t = 14.4 mm for the 0.97 kJ/mm GMAW pass and 22.3 mm for the 2.3 kJ/mm SAW pass. A 10 mm plate under the GMAW pass is 2-D (9.6 s), a 20 mm plate is 3-D (4.6 s). Above about 60 mm the thickness hardly matters any more.
What is t8/5 and how does EN 1011-2 calculate it?
t8/5 is the time a point spends cooling from 800 to 500 °C, the window where steel chooses between soft ferrite-pearlite and hard bainite or martensite. EN 1011-2 gives a 3-D and a 2-D formula in the heat input Q (kJ/mm), thickness d and start temperature T0; the greater value is the valid one. Shape factors correct for the joint: 1.0 for a bead on plate, 0.9 between passes of a butt weld, 0.67 for a single-run T fillet (its 2-D factor runs from 0.45 to 0.67 with heat input). Results can be off by up to 10 %. Fine-grain steels like 10 to 25 s; the book's GMAW butt pass gives 4.6 s, which is on the quick side.
How do you slow the cooling: heat input or preheat?
Both. In 3-D, t8/5 is proportional to Q, so halving the speed doubles it: the GMAW butt pass goes from 4.6 to 9.2 s at 3 mm/s. Preheating raises T0, which shrinks the temperature drop: at 150 °C the same pass takes 6.9 s, and at 100 °C 5.8 s. To get 10 s on the 20 mm butt joint the 2-D formula governs and you need Q = 1.98 kJ/mm, that is 2.94 mm/s (177 mm/min) at 28 V and 260 A. Too much heat input is not free: grain growth and toughness suffer.
On a thick plate you double the travel speed at the same volts and amps. What happens to the 3-D cooling time t8/5?
Q = k·U·I/v halves, and the 3-D time is proportional to Q. The butt pass goes from 4.62 s to 2.31 s. A thin plate would fall to a quarter, because the 2-D time goes with Q².
Worked examples
SAW flange pass: heat input, thickness regime, t8/5 · A 25 mm flange of the book's E350 plate (assumed) is welded by one SAW pass: 32 V, 600 A, 500 mm/min, thermal efficiency k = 1.0 (assumed procedure), no preheat (20 °C), between passes of a butt weld (F = 0.9).
- Speed v = 500/60 = 8.333 mm/s. Heat input Q = 1.0 × 32 × 600/(8.333 × 1000) = 2.304 kJ/mm.
- Transition thickness d_t = √[(4300 − 86) × 10⁵/6600 × Q × (1/480² − 1/780²)/(1/480 − 1/780)] = 22.3 mm. The plate is 25 mm, thicker, so 3-D.
- 3-D: t8/5 = 6600 × 2.304 × (1/480 − 1/780) × 0.9 = 10.97 s.
- Check the other formula: the 2-D value would be 8.69 s. The greater value is valid, so 10.97 s stands.
Answer: Q = 2.304 kJ/mm, 3-D flow, t8/5 = 11 s (inside the 10 to 25 s window).
Preheat and the GMAW butt pass · The 20 mm GMAW pass of the book (28 V, 260 A, 6 mm/s, k = 0.8, F = 0.9). The shop preheats and keeps the interpass at 150 °C. What is t8/5 and what regime is it?
- Q = 0.971 kJ/mm as before. With T0 = 150 °C: 3-D t8/5 = (6700 − 5 × 150) × Q × (1/350 − 1/650) × 0.9 = 6.85 s.
- Transition thickness at 150 °C: d_t = 16.2 mm, below 20 mm, so 3-D is right.
- For comparison, at 20 °C the value is 4.62 s: preheating to 150 °C stretches the cooling time by 48 %.
- At 100 °C it is 5.8 s, 26 % longer.
Answer: 6.85 s at 150 °C (3-D), up from 4.62 s.
Heat input and speed for t8/5 = 10 s on 20 mm · Same GMAW setting (28 V, 260 A, k = 0.8), 20 mm plate at 20 °C, butt pass (F = 0.9). The WPS asks for t8/5 of at least 10 s. What travel speed?
- Try 3-D only: Q = 10/(0.9 × 6600 × (1/480 − 1/780)) = 2.1 kJ/mm. But d_t at that Q is 21.2 mm, above 20 mm: the plate is thin for that heat input, so 2-D governs.
- 2-D: 10 = 0.9 × (4300 − 86) × 10⁵ × Q²/20² × (1/480² − 1/780²), so Q = 1.978 kJ/mm.
- Check: d_t = 20.6 mm > 20 mm, and the 3-D formula gives only 9.41 s, so the 2-D value (10 s) is the greater.
- v = k·U·I/(Q × 1000) = 0.8 × 28 × 260/(1.978 × 1000) = 2.94 mm/s = 177 mm/min.
Answer: Q = 1.98 kJ/mm, about 177 mm/min (the 6 mm/s pass is 2 times too fast).
Weld thermal cycles and the heat-affected zone of steel
Which syllabus covers thisAU CME395 Unit III (iron-iron carbide diagram, TTT and CCT diagrams, microstructural zones in welded plain-carbon steels)VTU not in syllabusSPPU 302045-A Unit 3 (concept of HAZ; pre- and post-weld heat treatment)MU not in syllabusKTU not in syllabus
What is a weld thermal cycle and what numbers describe it?
Pick a point in the plate and watch its temperature as the arc passes. It rises in a fraction of a second, reaches a peak, then falls slowly. Three numbers describe the cycle: the peak temperature, the time spent above a critical temperature, and the cooling rate (or t8/5). In the book's GMAW pass (assumed procedure) a point on the fusion line peaks at 1,500 °C. A point 1 mm outside it peaks at 1,011 °C and cools from 800 to 500 °C in 5.5 s. A point 2 mm outside peaks at 729 °C: it never reaches 800.
What are the zones of the heat-affected zone in a steel?
Peak temperature sorts the base metal into bands. Nearest the weld, above about 1,100 °C (assumed boundary), austenite grains grow big: the coarse-grained zone, with the lowest toughness. Between that and Ac3 (840 °C for the book's E350 plate) the steel is fully re-austenitised and cools to a fine grain. Between Ac3 and Ac1 (717 °C) it is only partly austenitised: the intercritical zone. Below Ac1 nothing transforms, and the old structure is only tempered. For the GMAW pass the three hot zones are 0.77, 0.78 and 0.51 mm wide: HAZ 2.1 mm. The same plate under the SAW pass has a 3.1 mm HAZ.
How does the iron-carbon diagram tell you what happens at each peak temperature?
In pure iron-carbon steel the eutectoid line A1 sits at 727 °C (0.76 % C) and the A3 line runs from 912 °C at zero carbon down to meet it. A steel below 0.76 % C starts to turn to austenite at A1 and finishes at A3. The book's E350 plate (0.17 % C, plus Mn and Si) has Ac1 = 717 °C and Ac3 = 840 °C by Andrews' equations, valid below 0.6 % C. Put 0.40 % C in and Ac3 falls to 795 °C: the intercritical band shrinks from 123 to 78 °C wide. Fast heating pushes the real temperatures higher.
How does cooling time choose the structure, and how hard can the HAZ get?
What the coarse-grained zone becomes depends on t8/5, as a CCT diagram shows (the Engineering Materials book has TTT and CCT). Quick cooling gives martensite or bainite; slow cooling gives ferrite and pearlite. A martensitic HAZ in this 0.17 % C steel could reach about HV 441 by the Düren relation (802 C + 305), above the ISO 15614-1 limit of 380 HV10 for an as-welded procedure test. That is why EN 1011-2 asks for t8/5 of 10 to 25 s on fine-grain steels. Preheat does it: 200 °C widens the GMAW HAZ from 2.05 to 2.8 mm (1.36 times) and slows the cooling.
What is acicular ferrite, and what does post-weld heat treatment do?
In the weld metal, the best structure for toughness is acicular ferrite: fine, interlocking plates that form inside the old austenite grains on small inclusions, so a crack has to change direction all the time. It forms at intermediate cooling rates, between the coarse grain boundary ferrite of slow cooling and the martensite of quick cooling. Post-weld heat treatment (PWHT) heats the whole joint to temper hard structures and relieve stress. It acts only below Ac1, here 717 °C, so it softens what the weld has hardened and never refines the coarse zone.
Preheat the plate to 200 °C and weld the same GMAW pass. What happens to the HAZ width (fusion line to Ac1)?
A hotter plate starts closer to Ac1 and loses heat more slowly. The model gives 2.05 mm at 20 °C and 2.8 mm at 200 °C, a factor 1.36. The pool grows too (4.3 to 4.6 mm half-width).
Worked examples
Peak temperature and zone 1 mm outside the fusion line · The GMAW pass on the book's 20 mm E350 plate (assumed): 28 V, 260 A, 6 mm/s, k = 0.8, plate at 20 °C. Use Rosenthal's 3-D solution with k = 24.1 W/m·K, ρc = 7.83 J/cm³·K (effective, matched to EN 1011-2). Find the fusion line, the peak at 1 mm outside it and the zone.
- Net power q = 0.8 × 28 × 260 = 5,824 W; q/v = 970.7 J/mm; a = k/ρc = 3.08 mm²/s.
- Fusion line: the lateral distance at which the peak just reaches 1,500 °C is 4.32 mm from the weld line.
- A point at 5.32 mm from the weld line peaks at 1,011 °C (golden-section search of T over time).
- Zone: 1,100 °C is reached out to 5.09 mm, so 1,011 °C lies between 1,100 °C and Ac3 = 840 °C: the fine-grained zone. t8/5 at that point is 5.5 s.
Answer: Peak 1,011 °C, fine-grained HAZ (FGHAZ), t8/5 = 5.5 s.
Width of the HAZ and the effect of heat input · Same plate, three of the book's procedures (assumed): SMAW 22 V, 110 A, 2 mm/s, k = 0.8; GMAW as above; SAW 32 V, 600 A, 500 mm/min, k = 1.0. Compare the HAZ widths (fusion line to Ac1 = 717 °C).
- Heat inputs: SMAW 0.97, GMAW 0.97, SAW 2.3 kJ/mm.
- Fusion line / Ac1 distances from the weld line: SMAW 3.75 / 5.89 mm; GMAW 4.32 / 6.37 mm; SAW 6.78 / 9.91 mm.
- HAZ width = Ac1 distance − fusion distance: SMAW 2.13 mm, GMAW 2.05 mm, SAW 3.13 mm.
- The SAW pass puts 2.4 times the heat into each millimetre but the HAZ is only 1.5 times wider: width goes slower than heat input.
Answer: SMAW 2.1 mm, GMAW 2.1 mm, SAW 3.1 mm.
Transformation temperatures and the hardness ceiling · THE STEEL (assumed heat analysis): C 0.17, Mn 1.35, Si 0.30, Cr 0.03, Mo 0.01, Ni 0.02, V 0.003 %. Find Ac1 and Ac3 (Andrews), then the same for 0.40 % C, and the martensite hardness of the 0.17 % C steel (Düren).
- Ac1 = 723 − 10.7 × 1.35 − 16.9 × 0.02 + 29.1 × 0.30 + 16.9 × 0.03 = 717.5 °C.
- Ac3 = 910 − 203 × √0.17 − 15.2 × 0.02 + 44.7 × 0.30 + 104 × 0.003 + 31.5 × 0.01 = 840 °C.
- At 0.40 % C: Ac3 = 795.3 °C, Ac1 unchanged at 717.5 °C (Ac1 does not depend on carbon in this relation).
- Martensite hardness HV = 802 × 0.17 + 305 = 441, against the 380 HV10 limit.
Answer: Ac1 717 °C, Ac3 840 °C; at 0.40 % C Ac3 is 795 °C; martensite would be about HV 441.
Weld pool solidification: epitaxial growth, G/R, grain structure and hot cracking
Which syllabus covers thisAU CME395 Unit III (phase transformations in weld and heat-affected zones, acicular ferrite and weld metal toughness)VTU not in syllabusSPPU 302045-A Unit 3 (weld thermal cycles)MU not in syllabusKTU not in syllabus
How do grains form in a weld, and why do they grow the way they do?
The weld metal freezes onto the base metal's own grains along the fusion line, with no new nuclei needed. That is epitaxial growth: each new grain copies the lattice of the grain it sits on. Then the grains compete. In a cubic metal the easy growth direction is along the cube edges, so the grains whose edges line up best with the heat flow, which is along the normal to the pool edge, crowd out the others. The result is long columnar grains that lean in the direction of travel and meet at the centreline. For the book's GMAW pool (8.6 mm wide, 27 mm long) the grains lean over a distance of tens of millimetres.
What are G and R, and what do G/R and G·R tell you?
G is the temperature gradient at the freezing front (K/mm). R is the speed the front advances (mm/s). The front grows along its own normal, so R = v·cos α, where α is the angle between the travel direction and that normal. On the centreline R = v; at the widest point R = 0. G/R sets the shape: high gives a plane front, then cells, then columnar dendrites, then equiaxed dendrites. G·R is the cooling rate and sets the fineness. For the GMAW pool, 60 % of the way out from the centreline: α = 72°, R = 1.83 mm/s, G = 183 K/mm, G/R = 100 K·s/mm², G·R = 335 K/s.
Why does the pool get longer and thinner at high speed, and why is that risky?
Faster travel at the same power puts less heat in each millimetre. The pool gets narrower, but the tail stretches. In Rosenthal's model the pool length-to-width ratio goes 2 at 2 mm/s, 3.2 at 6 and 4.3 at 12. The tail turns pointed, and the two sides of grains meet at a shallow angle on the centreline: the last liquid, rich in impurities, forms a thin film there. At the centreline G/R falls to 9.5 K·s/mm² at 6 mm/s and 4.7 at 12. Honest caveat: the real teardrop of a fast weld needs convection and latent heat, which this model leaves out.
What is solidification (hot) cracking and how do you avoid it?
As the last liquid freezes, sulphur and phosphorus collect in a thin film between the columnar grains. The film stays liquid below the bulk's freezing point, and contraction pulls the grains apart: a centreline crack. Steel specifications therefore limit both: IS 2062 allows at most 0.045 % S and 0.045 % P, and the book's E350 plate (assumed heat analysis) has 0.010 and 0.020. Cracking is worse for deep, narrow beads (depth greater than width), for high speed and for restraint. Cures: a wider, shallower bead, slower travel, a filler with more manganese to tie up sulphur, and low-impurity consumables. In the HAZ the same idea is called liquation cracking.
How can you refine the grain structure of a weld?
Finer grains are tougher and crack less. Faster cooling gives a finer structure: G·R rises from 342 K/s at 6 mm/s to 855 K/s at 15 mm/s on the centreline, though higher speed raises the cracking risk shown above. Better routes break the columnar growth: arc oscillation (weaving or magnetic) shifts the pool edge, pulsed current remelts the tips of the dendrites, and inoculants (titanium or aluminium compounds in the filler) give new nuclei so equiaxed grains form. Each one trades off against cost or penetration.
In the same pool, how does the growth rate R of the freezing front change from the fusion line (widest point) to the centreline?
R = v·cos α. At the widest point the edge normal is across the weld, so α = 90° and R = 0. At the centreline the normal points along the weld, α = 0 and R = v = 6 mm/s. At 60 % out we get α = 72°, R = 1.83 mm/s.
Worked examples
Growth rate and gradient at one point on the pool edge · The book's GMAW pool (28 V, 260 A, 6 mm/s, k = 0.8; effective steel k = 24.1 W/m·K, ρc = 7.83 J/cm³·K; model). Take the point on the rear edge of the 1,500 °C isotherm at 60 % of the half-width, y = 0.6 × the half-width.
- Half-width 4.32 mm, so y = 2.59 mm. The rear edge at that y is at ξ = −22.29 mm behind the arc (T = 1,500 °C there).
- Gradient of the Rosenthal field there: ∂T/∂ξ = 55.9 K/mm, ∂T/∂y = −174.2 K/mm, so G = 182.9 K/mm.
- Unit normal n = (∇T)/G = (0.305, −0.952); cos α = 0.305, α = 72.2°.
- R = v cos α = 6 × 0.305 = 1.83 mm/s; G/R = 100 K·s/mm²; G·R = 335 K/s.
Answer: R = 1.83 mm/s, G = 183 K/mm, G/R = 100 K·s/mm², G·R = 335 K/s.
The centreline: R = v, G from the cooling curve · Same pool, on the weld centreline just behind the arc, where the rear tip of the 1,500 °C isotherm sits at ξ = −25.97 mm (so q/(2πk|ξ|) = 1,480 K). Find R, G, G/R and the cooling rate G·R, and check G·R against the cooling-time formula.
- On the centreline T − T0 = q/(2πk|ξ|), so the gradient is (T − T0)/|ξ| = 1,480/25.97 = 57 K/mm.
- R = v = 6 mm/s (the tip moves with the arc, α = 0).
- G/R = 9.5 K·s/mm²; G·R = 342 K/s.
- Check: dT/dt at 1,500 °C from T − T0 = H/(2πk t) is (T − T0)² 2πk/H = 1,480² × 2π × 0.0241/971 = 342 K/s. They agree.
Answer: R = 6 mm/s, G = 57 K/mm, G/R = 9.5 K·s/mm², cooling rate 342 K/s.
Speed changes the pool shape and the centreline · Same power (5,824 W net) at 2, 6 and 12 mm/s. Compare pool length-to-width and the centreline G/R.
- Pool length / width (Rosenthal, 1,500 °C isotherm): 2.03 at 2 mm/s, 3.18 at 6 mm/s, 4.34 at 12 mm/s.
- Centreline G = (T − T0)/|ξ_tail| = q/(2πk|ξ|²): the tail tip sits where q/(2πk|ξ|) = 1,480 K whatever the speed, so G = 57, 57 and 57 K/mm: unchanged at fixed power.
- G/R = G/v: 28.5, 9.5 and 4.7 K·s/mm².
- So doubling the speed from 6 to 12 mm/s drops the centreline G/R by a factor 2: R doubles while G stays put, and the last liquid freezes at a lower G/R.
Answer: L/W 2 → 3.2 → 4.3; centreline G/R 28.5 → 9.5 → 4.7 K·s/mm².
Hydrogen cracking, carbon equivalents and preheat
Which syllabus covers thisAU CME395 Unit III (cold cracking, role of hydrogen and carbon equivalent)VTU BME302 Module 5 (weldability of materials)SPPU 302045-A Unit 3 (weldability and its assessment)MU not in syllabusKTU not in syllabus
What makes a steel weld crack with hydrogen, and when?
Three things have to be present together: hydrogen from the welding process, a hard, brittle structure in the HAZ (or weld metal) that is susceptible, and tensile stress on the joint. Remove any one and the crack does not form. It generally happens when the weld has cooled to about room temperature, and it rarely happens while the joint is still above ambient. That is why the cure is to keep the joint warm and let the hydrogen escape. For the book's E350 plate (assumed heat analysis) with CE = 0.407 the weld is borderline: CE below 0.4 is readily weldable, 0.4 to 0.5 needs care in thick sections.
Where does hydrogen come from, and how is it rated?
Moisture in flux and coatings, damp joints, oil, rust and the shielding gas all feed hydrogen into the pool. It is measured as diffusible hydrogen HD in ml per 100 g of deposited metal. EN 1011-2 gives scales: A above 15, B 10 to 15, C 5 to 10, D 3 to 5, E at most 3. Typical values: manual metal arc 5, MAG 3, basic flux-cored 5, basic submerged arc 5 ml/100 g (dry, basic consumables). The effect on preheat is large: for the E350 plate at 20 mm and 0.97 kJ/mm, going from HD 5 to HD 15 raises the CET-method preheat by 51 °C.
What are CE, CET and Pcm, and which one do you use?
A carbon equivalent squeezes the alloy content into one number for hardenability. CE(IIW) = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15 suits C-Mn steels and is the one in IS 2062. CET = C + (Mn+Mo)/10 + (Cr+Cu)/20 + Ni/40 is the one EN 1011-2 uses for its preheat equation. Pcm adds Si, V and boron and suits low-carbon steels. For the book's E350 plate: CE 0.407, CET 0.31, Pcm 0.253. IS 2062 limits CE to 0.47 for E350 grades A, BR and B0 (0.45 for grade C), so this plate passes, though CE 0.407 sits just above the 0.4 line.
How does EN 1011-2 calculate the preheat temperature?
Method B in EN 1011-2 gives the minimum preheat (also the interpass temperature) from the CET, the combined thickness d, the hydrogen HD and the heat input Q: Tp = 697 CET + 160 tanh(d/35) + 62 HD^0.35 + (53 CET − 32) Q − 328. It is valid for CET 0.2 to 0.5, d 10 to 90 mm, HD 1 to 20 and Q 0.5 to 4.0 kJ/mm, and outside that you must not trust it. The E350 plate at 20 mm with HD 5 and the GMAW pass (0.971 kJ/mm) needs 64 °C. At 50 mm it needs 124 °C. More heat input lowers it, by 15.6 °C per kJ/mm here.
What do you do on the shop floor beyond the preheat number?
Hold the joint warm after welding so the hydrogen escapes: TWI advises 2 to 3 hours at the preheat temperature for susceptible steels, and 250 to 300 °C for 3 to 4 hours for crack-sensitive cases (high CE, high restraint). Preheat up to 200 °C can be needed in thick high-CE steel. Keep consumables dry: bake low-hydrogen electrodes and use them from a holding oven. Where preheat is impractical an austenitic or nickel electrode keeps hydrogen locked in the weld metal. Weldability tests, such as the Tekken (Y-groove), CTS and implant tests, check a particular steel and procedure.
A 40 mm joint in the E350 plate is welded at 1 kJ/mm with HD 15 electrodes. Which single change cuts the CET-method preheat the most?
HD 15 to 5 lowers Tp by 51 °C. Doubling Q lowers it by only 16 °C (the term is (53 CET − 32) Q, and CET is 0.31). Welding faster lowers Q, which raises Tp. The combined thickness is a given.
Worked examples
Equivalents and preheat of a higher-alloy steel, 40 mm · An assumed higher-alloy structural steel (heat analysis invented for the example): C 0.22, Mn 1.45, Si 0.35, Cr 0.25, Mo 0.08, Ni 0.30, Cu 0.20, V 0.05 %. Combined thickness 40 mm, heat input 1.2 kJ/mm, HD 5 then 15.
- CE = 0.22 + 1.45/6 + (0.25 + 0.08 + 0.05)/5 + (0.30 + 0.20)/15 = 0.571. Over the IS 2062 E350 limit of 0.47, so it is not an E350 steel.
- CET = 0.22 + (1.45 + 0.08)/10 + (0.25 + 0.20)/20 + 0.30/40 = 0.403. Pcm = 0.342.
- Inside the CET method: CET 0.4 in 0.2 to 0.5, d = 40 in 10 to 90, Q = 1.2 in 0.5 to 4.0: yes.
- Tp = 697 × 0.403 + 160 tanh(40/35) + 62 × HD^0.35 + (53 × 0.403 − 32) × 1.2 − 328: 179 °C for HD 5, 231 °C for HD 15.
Answer: CE 0.571, CET 0.403; preheat 179 °C (HD 5) or 231 °C (HD 15).
THE STEEL: thickness, hydrogen and heat input · The book's E350 plate (CET 0.3095). Compare the CET-method preheat for 20 mm GMAW pass (Q 0.971), 50 mm GMAW pass, and 20 mm SAW pass (Q 2.304), all with HD 5.
- 20 mm GMAW: 697 × 0.3095 + 160 tanh(20/35) + 62 × 5^0.35 + (53 × 0.3095 − 32) × 0.971 − 328 = 64.1 °C.
- 50 mm GMAW: only d changes, tanh(50/35) = 0.891 against tanh(20/35) = 0.516: 124.1 °C.
- 20 mm SAW: (53 × 0.3095 − 32) = −15.6 per kJ/mm, so the larger Q = 2.304 gives 43.3 °C.
- With HD 15 the 20 mm GMAW case needs 115.2 °C, 51 °C more.
Answer: 64 °C (20 mm GMAW), 124 °C (50 mm), 43 °C (SAW), 115 °C (HD 15).
When the method does not apply · A lean steel, C 0.08, Mn 0.90, Si 0.30, Ni 0.02, Cu 0.03 %, thickness 8 mm, Q 0.97 kJ/mm, HD 5. Can you use the CET method?
- CET = 0.08 + 0.90/10 + 0.03/20 + 0.02/40 = 0.172, below the lower limit of 0.2.
- C 0.08 and Mn 0.90 are inside the method's composition ranges, but d = 8 mm is below the 10 mm lower limit.
- Two of the validity tests fail (CET and d). The formula would give −85 °C, which is below room temperature and meaningless.
- The honest answer is: use a table or guidance for thin, low-carbon steel, or do a weldability test.
Answer: No: CET 0.17 and d = 8 mm are both outside the method.
Welding stainless steels and dissimilar joints: Schaeffler diagram, sensitisation and sigma
Which syllabus covers thisAU CME395 Unit IV (welding of stainless steels: sensitisation, hot cracking, sigma phase, chromium carbide), Unit V (dissimilar materials)VTU not in syllabusSPPU 302045-A Unit 3 (welding of dissimilar materials, weld decay and sensitisation)MU not in syllabusKTU not in syllabus
What are the stainless steel families, and what does each ask of a welder?
Stainless steel is steel with chromium, which forms a thin film that stops rust. Austenitic grades (304, 316) hold 16-26 % Cr and 8-22 % Ni and weld easily, but crack if the weld metal has no ferrite. Ferritic grades (11-28 % Cr) grow coarse grains in the HAZ and lose toughness. Martensitic grades (12-18 % Cr) carry carbon, so the HAZ turns hard and cracks like a hardenable steel. Duplex grades (22-26 % Cr, 4-7 % Ni) need a heat input window, so the austenite and ferrite stay balanced. Source: TWI job knowledge.
How do you read the Schaeffler diagram for a weld?
Turn the weld's composition into two numbers: a chromium equivalent for the ferrite formers and a nickel equivalent for the austenite formers. Plot the point and read the region: austenite (A), austenite with ferrite (A+F), austenite with martensite (A+M), martensite (M) or ferrite (F). The book's 309L filler on 304 to E350 at 30 % dilution gives Cr_eq 19.9 and Ni_eq 13: A+F, ferrite 0 to 5 %. The diagram is a redrawn 1949 chart: good for the region, not a measurement.
Why does a stainless filler on carbon steel need a reserve of chromium and nickel?
The weld is a mix: filler times (1 − D) plus the melted base metals times D. Carbon steel adds almost no Cr and a lot of carbon, which counts 30 times in Ni_eq, so the point slides down and left towards martensite. With the book's analyses, 309L stays out of the A+M region until about 49 % dilution; 308L reaches it at about 16 %. Arc processes run 20-40 % dilution (SAW up to 80 %), so 309L is the filler for stainless to carbon steel. A buttering layer of 309L on the steel side first lowers the dilution in the final pass.
What is sensitisation (weld decay), and how do low carbon and stabilised grades avoid it?
Held in a band usually quoted as about 450-850 °C (a textbook range), chromium combines with carbon as carbide on the grain boundaries. The metal beside them is left short of chromium and corrodes along the boundaries: weld decay. The HAZ of 304 passes through that band on every weld. The fixes are less carbon (304L and 316L hold 0.03 % C at most, as does ER308L) or Ti or Nb to tie up the carbon first (321, 347). TWI notes that today's lower-carbon standard grades have made it far less common.
Why does a little ferrite help, and what goes wrong with too much?
A fully austenitic weld freezes in a way that pushes sulphur and phosphorus into the last liquid, which then tears open: solidification cracking. A few per cent of ferrite dissolves those impurities, and TWI calls 5-10 % ferrite extremely beneficial. Too much ferrite, held long at high temperature or cooled slowly in a high-alloy grade, turns into brittle sigma phase, an iron-chromium compound that costs toughness and corrosion resistance. So the aim is a band of a few per cent, not as much as possible, and low arc energies are avoided only as far as the grade allows.
A 304 plate is welded to E350 plate with ER308L at 30 % dilution. Where does the weld land on the Schaeffler diagram, and what is the cure?
308L gives Cr_eq 17.6 and Ni_eq 10, which is 1.4 Ni_eq units below the austenite boundary: austenite plus martensite. 309L at the same dilution is 3.4 units above it, and holds its reserve to 49 % dilution against 16 % for 308L.
Worked examples
Where does 309L land on 304 to E350? · A 304 plate is welded to the book's E350 plate. Filler ER309L (typical: C 0.02, Mn 1.5, Si 0.40, Cr 23.5, Ni 13.5, Mo 0.1). Both bases melt equally; dilution 30 %. 304 typical: C 0.04, Mn 1.2, Si 0.40, Cr 18.5, Ni 9.8, Mo 0.1.
- Equivalents of each: 304 Cr_eq = 18.5 + 0.1 + 1.5 × 0.4 = 19.2, Ni_eq = 9.8 + 30 × 0.04 + 0.5 × 1.2 = 11.6.
- E350 (C 0.17, Mn 1.35, Si 0.30): Cr_eq = 0.5, Ni_eq = 0.02 + 30 × 0.17 + 0.5 × 1.35 = 5.79. Filler 309L: Cr_eq 24.2, Ni_eq 14.8.
- Base mix is the mean of 304 and E350: Cr_eq 9.85, Ni_eq 8.7.
- Weld = 0.7 × filler + 0.3 × base mix: Cr_eq = 0.7 × 24.2 + 0.3 × 9.85 = 19.9; Ni_eq = 13.
- On the redrawn chart that point is in A+F (3.4 Ni_eq units above the martensite boundary), ferrite 0 to 5 %.
Answer: Cr_eq 19.9, Ni_eq 13: austenite with 0-5 % ferrite.
How much dilution can 309L or 308L take? · Same joint as before. The weld point moves in a straight line from the filler (D = 0) to the base mix (D = 1). Find the dilution at which it crosses the austenite / A+M boundary of the chart.
- Margin to the boundary (Ni_eq of the point minus the boundary at its Cr_eq) is linear in D: for 309L it is 8.6 at D = 0 and −8.85 at D = 1.
- It crosses zero at D = 8.6 / (8.6 − (−8.85)) = 0.493, so about 49 %.
- Repeating for 308L (D = 0 margin 1.74) gives 0.164, about 16 %.
- A normal GTAW or SMAW root at 20-40 % dilution therefore keeps 309L clear and not 308L; check the first pass, which dilutes most.
Answer: 309L to about 49 % dilution, 308L only to about 16 %.
Read a published dilution row · AWS Welding Journal's table for carbon steel (C 0.15, Mn 0.90, Si 0.10) welded to 304 with ER309/309L gives, at 40 % dilution, Cr 17.8 %, Ni 10.06 %, C 0.05 %, Mn 1.32 %, Si 0.34 %, Mo 0.08 %. Check one row and read it.
- Mix: Cr = 0.6 × 23.5 + 0.4 × (0 + 18.5)/2 = 17.8; Ni = 0.6 × 13.5 + 0.4 × (0 + 9.8)/2 = 10.06. Both agree with the table.
- Equivalents: Cr_eq = 17.8 + 0.08 + 1.5 × 0.34 = 18.4; Ni_eq = 10.06 + 30 × 0.05 + 0.5 × 1.32 = 12.2.
- Region: A (no ferrite): fine for strength, but no ferrite reserve against hot cracking.
- At 80 % dilution the same table gives Cr 12.1, Ni 6.62: Cr_eq 12.6, Ni_eq 9.6, region A+M.
Answer: 40 % row: Cr_eq 18.4, Ni_eq 12.2, region A; 80 % row falls to A+M.
Welding aluminium, copper, nickel, titanium and cast iron
Which syllabus covers thisAU CME395 Unit IV (welding of cast iron; joining of aluminium, copper, nickel and titanium alloys)VTU not in syllabusSPPU not in syllabusMU not in syllabusKTU not in syllabus
Why is aluminium hard to weld, and what is done about it?
Three things. A tough oxide film melts at 2,072 °C while the metal melts near 660 °C, so the film must be broken (AC TIG cleans it each half-cycle, or the wire is fed in a pulsed MIG arc). Liquid aluminium holds about 19 times more hydrogen than solid (0.65 against 0.034 ml per 100 g), so the freezing pool rejects gas as porosity. And the hot weld cracks: 4043 (Al-Si) and 5356 (Al-Mg) fillers are picked for the alloy. Clean, dry metal and wire matter most.
How does the same arc behave on steel, aluminium, copper and titanium?
Run the book's GTAW arc (864 W net, 1.5 mm/s) on each metal. Steel gives a pool 4.8 mm wide. Aluminium gives 2.7 mm and copper only 0.65 mm, because their conductivity carries the heat away. To match the steel pool, aluminium needs 1.8 times the power and copper 7.5 times. Titanium conducts badly and shows a pool 10 mm wide, but the table value (room temperature) overstates it. A first estimate only.
What makes copper and nickel alloys different at the weld?
Copper conducts about 16 times better than the book's effective steel, so heat leaves the joint almost as fast as it arrives: use a hotter, more concentrated source (helium or argon-helium shielding, GTAW or GMAW at high current) and preheat thick sections, with values from the procedure test. Nickel alloys such as 625 have a sluggish pool that does not wash out: place the filler, keep the joint clean and the heat input low, and keep sulphur out, since it makes nickel crack.
Why is titanium shielded so carefully, and what does the colour tell you?
Hot titanium takes up oxygen, nitrogen and hydrogen from the air and goes brittle. The pool, the HAZ and the back of the weld all need inert gas: a torch cup, a trailing shield and a back purge. TWI quotes a trailing shield held down to about 250 °C, and TIMET recommends shielding until below about 400 °C. The surface colour is a rough check: silver or light straw is acceptable, dark blue marginal, grey or white means rejected oxygen pick-up. TWI warns that colour is a poor indicator except when the contamination is gross.
Why does cast iron crack when welded, and what is the usual remedy?
Cast iron carries a few per cent carbon (about 2-4 %), which makes it hard, brittle and free of ductility. The weld pool's cooling, and the shrinkage, then crack the HAZ and the fusion boundary. The remedy is to reduce the cooling rate and the stress: preheat the whole casting (the temperature is set by the procedure test), weld in short stringers, peen each one while hot to relieve shrinkage, and use a nickel or nickel-iron electrode, whose soft deposit takes the strain. Buttering the faces first is common on repairs.
The book's GTAW arc makes a 4.8 mm wide pool in steel. How much net power does a copper plate of the same thickness need for the same pool width?
Copper's conductivity is 16 times the book's effective steel and its melting point is lower, 1,084 against 1,500 °C. Solving the Rosenthal pool for equal width gives 6,438 W against 864 W: 7.5 times. Aluminium needs 1.8 times.
Worked examples
Pool widths of the same arc · A GTAW arc of 864 W net (0.6 × 12 V × 120 A) moves at 1.5 mm/s on thick plate of steel, aluminium 6061, copper and Ti-6Al-4V. Properties: the kernel's table (steel k = 24.1 W/m·K effective; Al 180; Cu 394; Ti 6.7 at room temperature). Use the moving point-source (Rosenthal) pool at each melting point.
- Each pool is the surface isotherm at the melting point: steel 1,500 °C, Al 585 °C, Cu 1,084 °C, Ti 1,605 °C (solidus where known).
- Scanning the field T = T0 + q/(2πkR)·exp(−v(R + ξ)/2a) for its widest point gives half-widths: steel 2.41 mm, Al 1.33 mm, Cu 0.327 mm, Ti 5.15 mm.
- Widths are twice that: steel 4.81, Al 2.67, Cu 0.655, Ti 10.3 mm.
- The thin-plate (2-D) solution for aluminium at 20 mm never reaches 585 °C at all (heat spreads through the whole thickness too fast), so the thick-plate pool is the one that applies.
Answer: Steel 4.8 mm, aluminium 2.7 mm, copper 0.65 mm, titanium 10 mm (a first estimate).
Power for a steel-size pool · Same arc and speed. How much net power does an aluminium plate or a copper plate need to match the 4.81 mm steel pool?
- Pool width rises with power, so bisect on power until the half-width equals the steel's 2.406 mm.
- Aluminium: 1,575 W, which is 1,575/864 = 1.82 times the steel power.
- Copper: 6,438 W = 7.45 times.
- Titanium needs only 269 W (0.31 times) in this table, but its conductivity roughly triples when hot, so that is too low.
Answer: Aluminium 1,575 W (1.8 ×), copper 6,438 W (7.5 ×).
How much porosity could the hydrogen make? · A 100 g aluminium weld pool (assumed) is saturated with hydrogen at 660 °C: 0.65 ml per 100 g liquid, 0.034 ml per 100 g solid (patent summary). Aluminium density 2.7 g/cm³. Every bubble stays in the metal; gas volumes counted at standard conditions (hot gas trapped in a freezing pool takes up about 3.4 times more, 933 K against 273 K).
- Gas rejected on freezing = (0.65 − 0.034) ml per 100 g × 100 g = 0.616 ml.
- Metal volume = 100 g / 2.7 g/cm³ = 37 cm³.
- Porosity = 0.616 / 37 = 1.66 % by volume.
- Solubility rises further as the pool gets hotter (the fit log S = −2980/T + 3.07 gives 0.75 ml/100 g at 933 K), so a hot pool is worse than this.
Answer: Up to about 1.7 % porosity by volume, from the hydrogen alone: that is why wire and plate must be clean and dry.
Residual stress and distortion: shrinkage, angular distortion and how to control them
Which syllabus covers thisAU not in syllabusVTU BME302 Module 5 (distortion, shrinkage and residual stresses in welded structures)SPPU 302045-A Unit 3 (effects of pre- and post-weld heat treatment)MU not in syllabusKTU not in syllabus
Why does a weld shrink and leave stress behind?
The weld and the metal beside it are heated near 1,500 °C and try to expand, but the cold plate around them holds them. They are squashed and flow plastically. On cooling they try to contract by about α ΔT = 12e-6 (typical) × 1,480 = 1.8 %, and the cold plate holds them again. The result is a strip of weld metal and HAZ left in tension, up to the yield strength, with the rest of the plate squeezed in balance. The part also shortens and bends: that is distortion. Take away the restraint and you get distortion; keep it and you get stress.
How do the stress across a weld, the shrinkage and the angle come from the groove?
Stress along the weld follows the Masubuchi-Martin curve: tension up to the yield (350 MPa for E350) in a zone about b = 10 mm each side of the centreline, balanced by compression of up to 156 MPa farther out. Transverse shrinkage is S = 0.2 Aw/t + 0.05 d: the book's 20 mm single-V (Aw 261 mm²) shrinks 2.7 mm. More metal on one face rotates the plates: a model of the layers gives up to 13° for the single-V and zero for a symmetric double-V.
What types of distortion are there?
Transverse shrinkage: the plates move together across the weld. Longitudinal shrinkage: the weld shortens along its length (TWI quotes about 0.8 mm per 3 m of fillet weld and 3 mm per 3 m of butt weld). Angular distortion: the plates rotate because the weld is bigger on one face, as in a single-V butt or a one-sided fillet. Bowing: a long member bends because the weld sits off its neutral axis. Buckling: thin plate goes wavy where the compressive residual stress exceeds its buckling stress. TWI adds that shrinkage cannot be predicted accurately.
How do you control distortion in the shop?
Put in less weld metal: the double-V above has 175 mm² against 261 mm² for the single-V, a third less shrinkage (1.8 mm against 2.7), and weld alternate sides to balance it. Use smaller fillets, intermittent welds, back-step and skip sequences, and fewer, larger passes where the joint allows. Preset the plates by the angle you expect, jig and clamp them, or leave the parts to cool in the fixture. For the single-V the model asks for 6.4° per plate: a ceiling, since tack welds and clamps already hold some of it.
How is residual stress relieved, and what does it do to the part?
Post-weld heat treatment heats the whole fabrication to a code temperature (for C-Mn steel usually near 600 °C, set by the construction code) and holds it, so creep relaxes the stress; it also tempers hard HAZ zones. Mechanical methods are lighter: peening cold-works the weld surface into compression, and vibratory stress relief is used on castings and frames. Residual tension adds to the service load in fatigue and stress corrosion cracking, and compression in the plate lowers the buckling strength, so heavy and cyclic structures are relieved. The temperatures are typical values: use the code.
A 20 mm plate is welded with a 60° single-V and then with a 60° double-V, both with a 2 mm gap and a 2 mm root face. Which statement is right?
Metal per metre: single-V 261 mm², double-V 175 mm². Shrinkage 2.71 mm against 1.85 mm. In the layer model the single-V rotates up to 13° and a symmetric double-V zero, because the two faces shrink alike.
Worked examples
Transverse shrinkage of the book's joint · The book's 20 mm single-V (60°, 2 mm gap, 2 mm root face, 2 mm cap): groove fill 227.1 mm², with the cap 261.4 mm². Find the transverse shrinkage with S = 0.2 Aw/t + 0.05 d, and the same for a double-V.
- Single-V: S = 0.2 × 261.4/20 + 0.05 × 2 = 2.614 + 0.1 = 2.71 mm.
- Double-V (fill 133.5 mm², with two caps 174.6 mm²): S = 0.2 × 174.6/20 + 0.1 = 1.85 mm.
- Check against TWI's 1.5-3 mm per 60° butt weld: both lie inside; the double-V saves 0.87 mm (32 %).
- Allow 2.7 mm in the cutting length of each plate pair, then trial-weld: TWI warns that it is almost impossible to predict shrinkage accurately.
Answer: 2.71 mm for the single-V, 1.85 mm for the double-V.
Stress across the weld · E350 plate up to 20 mm: yield 350 MPa (IS 2062). A GMAW pass (net 5,824 W at 6 mm/s) puts the tension zone's edge where the peak temperature is 20 + 2σy/(Eα) = 298 °C (E = 210 GPa, α = 12e-6 per K, typical). Use σ(y) = σ0[1 − (y/b)²]e^(−y²/2b²).
- Edge temperature: 2 × 350/(2,10,000 × 12e-6) = 278 K above room, so 298 °C.
- The Rosenthal peak at that temperature is at b = 10.2 mm from the centreline.
- At y = 0 the stress is 350 MPa; it crosses zero at y = b = 10.2 mm.
- The most compressive point is y = √3 b = 17.6 mm, σ = −2 e^(−1.5) × 350 = −156 MPa; at y = 2b it is −3 e^(−2) × 350 = −142 MPa.
- Integrated over a 300 mm plate, tension 4.32 kN/mm balances compression 4.32 kN/mm: the profile self-balances.
Answer: b = 10.2 mm; tension to 350 MPa, compression to −156 MPa, balanced at 4.3 kN/mm.
Angle of a single-V and the presetting · Same joint. Model: each layer shrinks by 0.2 × (its groove width); plane sections stay plane; the plates close by the least-squares slope of that shrinkage over the thickness.
- Layer widths: 22.8 mm at the top, falling to 2 mm over the 18 mm bevel depth, then 2 mm through the root face.
- Shrinkage per layer = 0.2 × width: 4.56 mm at the top, 0.4 mm at the root.
- Slope by regression on 4000 layers = −0.2245 mm per mm, so the plates close by 0.224 rad = 12.9°.
- Preset each plate by half of it: 6.4°. The double-V (symmetric) gives slope 0, so no presetting.
- This is a free-plate ceiling: tacks and clamps cut it, so the preset is found by a trial weld.
Answer: Up to 13° free rotation for the single-V (preset 6.4° a plate); zero for a symmetric double-V.
Weld defects, inspection and codes: NDT, weldability tests, WPS, PQR and welder qualification
Which syllabus covers thisAU CME395 Unit V (defects in welded joints, weldability and testing of weldments, international standards and codes)VTU BME302 Module 5 (welding defects and remedies)SPPU 302045-A Unit 3 (weld characterisation; ASME, AWS and IS welding standards, welding skill levels)MU not in syllabusKTU not in syllabus
What are the common weld defects, their causes and their remedies?
Porosity: gas in the pool from damp, oily or rusty metal or a draughty shield. Clean it, dry the consumables, fix the gas flow. Slag inclusion: slag trapped between passes; clean each pass. Lack of fusion: weld metal not melted into the wall or the pass below, from low current or poor technique; raise heat input, mind the angle. Incomplete penetration: the root is not filled; open the gap, reduce the root face. Undercut: a groove melted into the plate from too much current or speed. Cracks: hot (in the weld, from the pool) or cold (hydrogen, in the HAZ): never allowed. Arc strikes: hard spots to grind out.
What do visual, dye penetrant and magnetic particle testing find?
Visual inspection comes first: with a gauge and good light it finds undercut, bad profile, spatter and some cracks, and costs almost nothing. Dye penetrant (PT) finds cracks and pores open to the surface on any non-porous metal, including stainless and aluminium: red or fluorescent dye is drawn into the crack and shown by a developer. Magnetic particle (MT) finds surface and just-subsurface cracks in ferromagnetic steel only, by iron powder gathering where a crack leaks the magnetic field. Both leave the inside of a thick weld unchecked.
How do ultrasonic and radiographic testing find flaws inside a weld, and which finds what best?
An angle-beam probe sends shear waves (about 3,230 m/s in steel) at 45, 60 or 70° and the echo's sound path s locates the flaw: depth = s cos θ on the first leg, 2t − s cos θ on the second. In a 20 mm plate a 60° beam skips every 69.3 mm. UT finds flat flaws such as cracks and lack of fusion best; radiography (RT) shows volume flaws such as pores and slag as a picture, but a tight crack at the wrong angle can vanish. RT's sharpness is limited by Ug = F t/D: 0.1 mm for a 3 mm source at 600 mm.
What are the ISO 5817 quality levels?
ISO 5817 grades a weld's imperfections as level B (the strictest), C or D. Cracks are not permitted at any level. For undercut on plate over 3 mm, D allows a depth of 0.2 t up to 1 mm, C 0.1 t up to 0.5 mm, B 0.05 t up to 0.5 mm: for the 20 mm plate that is 1, 0.5 and 0.5 mm. Uniform porosity in one layer is limited to 2.5 % (D), 1.5 % (C) and 1 % (B) of the projected area. The level is chosen by the design or the product code, not by the inspector.
What are a WPS, a PQR and a welder qualification, and which code covers which?
A welding procedure specification (WPS) is the recipe: process, consumables, current, heat input, preheat. A procedure qualification record (PQR) is the proof: the test weld made to that recipe with its tensile, bend, impact and hardness results. A welder qualifies separately by a test weld in a position and range. ISO 15614-1 qualifies steel procedures and ISO 9606-1 welders; ASME IX covers both procedures and welders only (ASME VIII and others say what to build); AWS D1.1 is a structural steel code that covers fabrication, inspection and qualification. Indian practice follows BIS codes such as IS 816 and IS 9595: check the current edition.
A 60° probe sits 57.5 mm from the weld centre on the 20 mm plate and the A-scan shows an echo at a sound path of 60 mm. Where is the flaw?
A 60 mm path is longer than the first leg to the back wall (40 mm), so the beam has reflected. Depth = 2t − s cos θ = 40 − 60 × 0.5 = 10 mm. The beam has travelled 52 mm along the surface from the probe index, so the flaw is 57.5 − 52 = 5.5 mm from the centre: the side wall of the V.
Worked examples
Skip distance and where to stand · A 20 mm plate is scanned with 45°, 60° and 70° shear probes. Find the full skip, the half skip and the probe position at which a side-wall flaw 10 mm deep, 5.6 mm from the weld centreline, is met on each leg (60° probe, beam half width ignored).
- Full skip = 2 t tan θ: 45° = 40 mm, 60° = 69.3 mm, 70° = 109.9 mm; half skip is half of that.
- First leg meets the flaw when X = x + d tan θ = 5.62 + 10 × tan 60° = 22.9 mm.
- Second leg: X = x + (2t − d) tan θ = 5.62 + 30 × tan 60° = 57.6 mm.
- Sound path: first leg d/cos θ = 20 mm, second leg (2t − d)/cos θ = 60 mm; round-trip time 37.2 µs at 3,230 m/s.
- The bevel face is 30° from the vertical, so the second leg of a 60° beam hits it square on (cosine of the angle 1) and the first leg at 60° off (0.5): scan the second leg for side-wall flaws.
Answer: Skips 40, 69.3, 109.9 mm; stand at 22.9 mm (first leg) or 57.6 mm (second leg).
Locate the flaw from the echo · 60° probe, index 57.5 mm from the weld centreline on the 20 mm plate. The scope shows an echo at sound path 60 mm.
- First-leg path to the back wall = t/cos θ = 40 mm. The echo path is longer, so it is on the second leg.
- Depth = 2t − s cos θ = 40 − 60 × 0.5 = 10 mm.
- Distance along the surface from the index = s sin θ = 60 × 0.866 = 52 mm.
- Flaw position from the weld centre = 57.5 − 52 = 5.5 mm, on the side wall (5.6 mm at that depth): lack of side-wall fusion.
Answer: 10 mm deep, 5.5 mm from the weld centreline: side-wall lack of fusion.
Radiographic unsharpness · Radiography of the 20 mm weld with a 3 mm source. The film is against the back face; the ASME V guide (0.020 in for material up to 2 in) is 0.508 mm.
- Ug = F t / D = 3 × 20/600 = 0.1 mm at D = 600 mm: inside the limit.
- Minimum distance for the limit = F t / Ug = 3 × 20/0.508 = 118 mm.
- At D = 150 mm the same source gives 0.4 mm, which is 0.8 times the limit: still allowed, but crack edges blur four times as much as at 600 mm.
- A bigger source or thicker plate needs a longer distance, so the exposure time grows as D squared.
Answer: Ug = 0.1 mm at 600 mm; at least 118 mm is needed for the 0.51 mm limit.
Keep going
- Manufacturing Processes interactive book
- Engineering Materials and Metallurgy interactive book
- Design of Machine Elements interactive book
- Machine Drawing interactive book
- All Skill-Lync interactive books
Recommended reading
- Welding Engineering and Technology, R. S. Parmar
- Welding Processes and Technology, R. S. Parmar
- Welding Metallurgy, Sindo Kou
- Welding Technology for Engineers, Baldev Raj, V. Shankar and A. K. Bhaduri
- Welding and Welding Technology, Richard L. Little
- Advanced Welding Processes, John Norrish
How this book was made
Chapters follow the official syllabi listed above. Every interactive's formulas and every worked-example number were checked by script. Explanations, animations and examples are original to Skill-Lync.